Henley's Twentieth Century Formulas, Recipes and Processes
3,571,313 chars · English
The Project Gutenberg eBook of Henley's Twentieth Century Formulas, Recipes and Processes
This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.
Title: Henley's Twentieth Century Formulas, Recipes and Processes
Editor: Gardner Dexter Hiscox
Release date: September 25, 2016 [eBook #53143]
Most recently updated: October 23, 2024
Language: English
Other information and formats: www.gutenberg.org/ebooks/53143
Credits: Produced by Brian Coe, RichardW, and the Online Distributed
Proofreading Team at http://www.pgdp.net (This file was
produced from images generously made available by University
of California libraries, and by archive.org)
*** START OF THE PROJECT GUTENBERG EBOOK HENLEY'S TWENTIETH CENTURY FORMULAS, RECIPES AND PROCESSES ***
«HENLEY’S TWENTIETH CENTURY RECIPES, FORMULAS AND PROCESSES»
CONTAINING TEN THOUSAND SELECTED HOUSEHOLD AND WORKSHOP FORMULAS,
RECIPES, PROCESSES AND MONEY-SAVING METHODS FOR THE PRACTICAL USE OF
MANUFACTURERS, MECHANICS, HOUSEKEEPERS AND HOME WORKERS
EDITED BY
GARDNER D. HISCOX, M.E.
AUTHOR OF “MECHANICAL MOVEMENTS, POWERS AND DEVICES,” “COMPRESSED
AIR,” “GAS, GASOLINE AND OIL ENGINES,” ETC., ETC.
[Illustration]
1914 EDITION, REVISED AND ENLARGED
NEW YORK
THE NORMAN W. HENLEY PUBLISHING COMPANY
132 NASSAU STREET
1914
COPYRIGHT, 1914 AND 1913, BY
THE NORMAN W. HENLEY PUBLISHING COMPANY
COPYRIGHT, 1912 AND 1907, BY
THE NORMAN W. HENLEY PUBLISHING COMPANY
Also, Entered at Stationers’ Hall Court, London, England
_All rights reserved_
THE TROW PRESS, NEW YORK
«PREFACE»
In compiling this book of formulas, recipes and processes, the Editor
has endeavored to meet the practical requirements of the home and
workshop—the mechanic, the manufacturer, the artisan, the housewife,
and the general home worker.
In addition to exercising the utmost care in selecting his materials
from competent sources, the Editor has also modified formulas which
were obviously ill adapted for his needs, but were valuable if altered.
Processes of questionable merit he has discarded. By adhering to this
plan the Editor trusts that he has succeeded in preparing a repository
of useful knowledge representing the experience of experts in every
branch of practical achievement. Much of the matter has been specially
translated for this work from foreign technological periodicals and
books. In this way the Editor has embodied much practical information
otherwise inaccessible to most English-speaking people.
Each recipe is to be regarded as a basis of experiment, to be modified
to suit the particular purpose in hand, or the peculiar conditions
which may affect the experimenter. Chemicals are not always of uniform
relative purity and strength; heat or cold may markedly influence the
result obtained, and lack of skill in the handling of utensils and
instruments may sometimes cause failure. Inasmuch as a particular
formula may not always be applicable, the Editor has thought it
advisable to give as many recipes as his space would allow under
each heading. In some instances a series of formulas is given which
apparently differ but slightly in their ingredients. This has been done
on the principle that one or more may be chosen for the purpose in hand.
Recognizing the fact that works of a similar character are not unknown,
the Editor has endeavored to present in these pages the most modern
methods and formulas. Naturally, old recipes and so-called trade
secrets which have proven their value by long use are also included,
particularly where no noteworthy advance has been made; but the primary
aim has been to modernize and bring the entire work up to the present
date.
THE EDITOR.
JANUARY, 1914.
«PARTIAL LIST OF AUTHORITIES CONSULTED»
Apothecary, The.
Berliner Drog. Zeitung.
Brass World.
British Journal of Photography.
Chemical News.
Chemiker Zeitung Repertorium.
Chemisch Technische Fabrikant.
Chemische Zeitung.
Chemist-Druggist.
Comptes Rendus.
Cooley’s Receipts.
Cosmos.
Dekorationsmaler, Der.
Deutsche Drog. Zeitung.
Deutsche Goldschmiede Zeitung.
Deutsche Handwerk.
Deutsche Maler Zeitung.
Deutsche Topfer und Ziefler Zeitung.
Dingler’s Polytechnic Journal.
Drogisten Zeitung.
Druggists’ Circular.
English Mechanic.
Farben Zeitung.
Gummi Zeitung.
Journal der Goldschmiedekunst.
Journal of Applied Microscopy.
Journal of the Franklin Institute.
Journal Society of Chemical Industry.
Journal Suisse d’Horlogerie.
Keramische Rundschau.
La Nature.
La Science en Famille.
La Vie Scientifique.
Lack und Farben Industrie.
Legierungen.
Le Genie Civil.
Le Praticien.
Leipziger Farber und Zeugdrucker Zeitung.
Maler Zeitung.
Metallarbeiter.
Mining and Scientific Press.
Neueste Erfindungen und Erfahrungen.
Nouvelles Scientifiques.
Oils, Colors, and Drysalteries.
Papier-Zeitung.
Parfumer, Der.
Pharmaceutische Zeitung.
Pharmaceutische Centralhalle.
Pharmaceutische Era.
Pharmaceutische Journal.
Pharmaceutische Journal Formulary.
Photo Times.
Polytech. Centralblatt.
Polyt. Notizblatt.
Popular Science News.
Pottery Gazette.
Practical Druggist.
Revue Chronometrique.
Revue de la Droguerie.
Revue des Produits Chimiques.
Revue Industrielle.
Science, Arts and Nature.
Science Pratique.
Seifensieder Zeitung, Der.
Seifenfabrikant, Der.
Spatula.
Stein der Weisen, Der.
Sudd. Apoth. Zeitung.
Technisches Centralblatt.
Technische Rundschau.
Uhland’s Technische Rundschau.
Verzinnen Verzinken Vernickeln, Das.
Werkmeister Zeitung.
Wiener Drogisten Zeitung.
Wiener Gewerbe Zeitung.
Zeitschrift für die Gesammte Kohlensaure Industrie.
{9}
«HENLEY’S BOOK OF RECIPES»
ABRASION REMEDY: See Cosmetics and Ointments.
ABSINTHE: See Wines and Liquors.
«Acid-Proofing»
«An Acid-Proof Table Top.»—
1.
Copper sulphate 1 part
Potassium chlorate 1 part
Water 8 parts
Boil until salts are dissolved.
2.
Aniline hydrochlorate 3 parts
Water 20 parts
Or, if more readily procurable:
Aniline 6 parts
Hydrochloric acid 9 parts
Water 50 parts
By the use of a brush two coats of solution No. 1 are applied while
hot; the second coat as soon as the first is dry. Then two coats of
solution No. 2, and the wood allowed to dry thoroughly. Later, a coat
of raw linseed oil is to be applied, using a cloth instead of a brush,
in order to get a thinner coat of the oil.
A writer in the _Journal of Applied Microscopy_ states that he has used
this method upon some old laboratory tables which had been finished in
the usual way, the wood having been filled oiled, and varnished. After
scraping off the varnish down to the wood, the solutions were applied,
and the result was very satisfactory.
After some experimentations the formula was modified without materially
affecting the cost, and apparently increasing the resistance of the
wood to the action of strong acids and alkalies. The modified formula
follows:
1.
Iron sulphate 4 parts
Copper sulphate 4 parts
Potassium permanganate 8 parts
Water, q. s. 100 parts
2.
Aniline 12 parts
Hydrochloric acid 18 parts
Water, q. s. 100 parts
Or:
Aniline hydrochlorate 15 parts
Water, q. s. 100 parts
Solution No. 2 has not been changed, except to arrange the parts per
hundred.
The method of application is the same, except that after solution No. 1
has dried the excess of the solution which has dried upon the surface
of the wood is thoroughly rubbed off before the application of solution
No. 2. The black color does not appear at once, but usually requires a
few hours before becoming ebony black. The linseed oil may be diluted
with turpentine without disadvantage, and after a few applications the
surface will take on a dull and not displeasing polish. The table tops
are easily cleaned by washing with water or suds after a course of work
is completed, and the application of another coat of oil puts them in
excellent order for another course of work. Strong acids or alkalies
when spilled, if soon wiped off, have scarcely a perceptible effect.
A slate or tile top is expensive not only in its original cost, but
also as a destroyer of glassware. Wood tops when painted, oiled, or
paraffined have objectionable features, the latter especially in warm
weather. Old table tops, after the paint or oil is scraped off down to
the wood, take the above finish nearly as well as the new wood.
«To Make Wood Acid- and Chlorine-Proof.»—Take 6 pounds of wood tar and
12 pounds rosin, and melt them together in an iron kettle, after which
stir in 8 pounds finely powdered brick dust. The damaged parts must be
cleaned perfectly and dried, whereupon they may be painted over with
the warm preparation or filled up and drawn off, leaving the film on
the inside.
«Protecting Cement Against Acid.»—A paint to protect cement against
acid is obtained by mixing pure asbestos, very finely powdered,
with a thick solution of {10} sodium silicate. The sodium silicate
must be as alkaline as possible. The asbestos is first rubbed with
a small quantity of the silicate, until a cake is obtained and then
kept in well-closed vessels. For use this cake is simply thinned with
a solution of the silicate, which furnishes a paint two or three
applications of which protect the walls of reservoirs, etc., against
any acid solid or liquid. This mass may also be employed for making a
coating of sandstone.
«To Make Corks Impermeable and Acid-Proof.»—Choose your corks
carefully. Then plunge them into a solution of gelatin or common glue,
15 parts, in 24 parts of glycerine and 500 parts of water, heated to
44° or 48° C. (112°–120° F.), and keep them there for several hours. On
removing the corks, which should be weighted down in the solution, dry
them in the shade until they are free from all surplus moisture. They
are now perfectly tight, retaining at the same time the greater portion
of their elasticity and suppleness. To render them acid-proof, they
should be treated with a mixture of vaseline, 2 parts, and paraffine
7 parts, heated to about 105° F. This second operation may be avoided
by adding to the gelatin solution a little ammonium dichromate and
afterwards exposing the corks to the light.
«Lining for Acid Receptacles.»—Plates are formed of 1 part of brown
slate, 2 of powdered glass, and 1 of Portland cement, the whole worked
up with silicate of soda, molded and dried. Make a cement composed of
ground slate and silicate of soda and smear the surface for the lining;
then, while it is still plastic, apply the plates prepared as above
described. Instead of these plates, slabs of glass or porcelain or
similar substances may be employed with the same cement.
ACACIA, MUCILAGE OF: See Adhesives under Mucilages.
ACID-PROOF GLASS: See Glass.
ACID-RESISTING PAINT: See Paint.
ACIDS, SOLDERING: See Solders.
ACID STAINS FROM THE SKIN, TO REMOVE: See Cleaning Preparations and
Methods.
ACID TEST FOR VINEGAR: See Vinegar.
«Adhesives»
«GLUES:»
«Manufacture of Glue.»—I.—The usual process of removing the phosphate
of lime from bones for glue-making purposes by means of dilute
hydrochloric acid has the disadvantage that the acid cannot be
regenerated. Attempts to use sulphurous acid instead have so far proved
unsuccessful, as, even with the large quantities used, the process
is very slow. According to a German invention this difficulty with
sulphurous acid can be avoided by using it in aqueous solution under
pressure. The solution of the lime goes on very rapidly, it is claimed,
and no troublesome precipitation of calcium sulphite takes place. Both
phosphate of lime and sulphurous acid are regenerated from the lyes by
simple distillation.
II.—Bones may be treated with successive quantities of combined
sulphurous acid and water, from which the heat of combination has been
previously dissipated, the solution being removed after each treatment,
before the bone salts dissolved therein precipitate, and before the
temperature rises above 74° F.—U. S. Pat. 783,784.
III.—A patent relating to the process for treating animal sinews,
preparatory for the glue factory, has been granted to Florsheim,
Chicago, and consists in immersing animal sinews successively in
petroleum or benzine to remove the outer fleshy animal skin; in
a hardening or preserving bath, as boric acid, or alum or copper
sulphate; and in an alkaline bath to remove fatty matter from the
fibrous part of the sinews. The sinews are afterwards tanned and
disintegrated.
«Test for Glue.»—The more water the glue takes up, swelling it, the
better it is. Four ounces of the glue to be examined are soaked for
about 12 hours in a cool place in 4 pounds of cold water. If the glue
has dissolved after this time, it is of bad quality and of little
value; but if it is coherent, gelatinous, and weighing double, it is
good; if it weighs up to 16 ounces, it is very good; if as much as 20
ounces, it may be called excellent.
«To Prevent Glue from Cracking.»—To prevent glue from cracking, which
frequently occurs when glued articles are {11} exposed to the heat of a
stove, a little chloride of potassium is added. This prevents the glue
from becoming dry enough to crack. Glue thus treated will adhere to
glass, metals, etc., and may also be used for pasting on labels.
«Preventing the Putrefaction of Strong Glues.»—The fatty matter always
existing in small quantity in sheets of ordinary glue affects the
adhesive properties and facilitates the development of bacteria, and
consequently putrefaction and decomposition. These inconveniences are
remedied by adding a small quantity of caustic soda to the dissolved
glue. The soda prevents decomposition absolutely; with the fatty matter
it forms a hard soap which renders it harmless.
«Liquid Glues.»—
I.—Glue 3 ounces
Gelatin 3 ounces
Acetic acid 4 ounces
Water 2 ounces
Alum 30 grains
Heat together for 6 hours, skim, and add:
II.—Alcohol 1 fluid ounce
Brown glue, No. 2. 2 pounds
Sodium carbonate 11 ounces
Water 3 1/2 pints
Oil of clove 160 minims
Dissolve the soda in the water, pour the solution over the dry glue,
let stand over night or till thoroughly soaked and swelled, then heat
carefully on a water bath until dissolved. When nearly cold stir in the
oil of cloves.
By using white glue, a finer article, fit for fancy work, may be made.
III.—Dissolve by heating 60 parts of borax in 420 parts of water,
add 480 parts dextrin (pale yellow) and 50 parts of glucose and heat
carefully with continued stirring, to complete solution; replace the
evaporated water and pour through flannel.
The glue made in this way remains clear quite a long time, and
possesses great adhesive power; it also dries very quickly, but upon
careless and extended heating above 90° C. (194° F.), it is apt to turn
brown and brittle.
IV.—Pour 50 parts of warm (not hot) water over 50 parts of Cologne glue
and allow to soak over night. Next day the swelled glue is dissolved
with moderate heat, and if still too thick, a little more water is
added. When this is done, add from 2 1/2 to 3 parts of crude nitric
acid, stir well, and fill the liquid glue in well-corked bottles. This
is a good liquid steam glue.
V.—Soak 1 pound of good glue in a quart of water for a few hours, then
melt the glue by heating it, together with the unabsorbed water, then
stir in 1/4 pound dry white lead, and when that is well mixed pour in
4 fluidounces of alcohol and continue the boiling 5 minutes longer.
VI.—Soak 1 pound of good glue in 1 1/2 pints of cold water for
5 hours, then add 3 ounces of zinc sulphate and 2 fluidounces of
hydrochloric acid, and keep the mixture heated for 10 or 12 hours at
175° to 190° F. The glue remains liquid and may be used for sticking a
variety of materials.
VII.—A very inexpensive liquid glue may be prepared by first soaking
and then dissolving gelatin in twice its own weight of water at a very
gentle heat; then add glacial acetic acid in weight equal to the weight
of the dry gelatin. It should be remembered, however, that all acid
glues are not generally applicable.
VIII.—Glue 200 parts
Dilute acetic acid 400 parts
Dissolve by the aid of heat and add:
Alcohol 25 parts
Alum 5 parts
IX.—Glue 5 parts
Calcium chloride 1 part
Water 1 part
X.—Sugar of lead 1 1/2 drachms
Alum 1 1/2 drachms
Gum arabic 2 1/2 drachms
Wheat flour 1 av. lb.
Water, q. s.
Dissolve the gum in 2 quarts of warm water; when cold mix in the flour,
and add the sugar of lead and alum dissolved in water; heat the whole
over a slow fire until it shows signs of ebullition. Let it cool, and
add enough gum water to bring it to the proper consistence.
XI.—Dilute 1 part of official phosphoric acid with 2 parts of water and
neutralize the solution with carbonate of ammonium. Add to the liquid
an equal quantity of water, warm it on a water bath, and dissolve in it
sufficient glue to form a thick syrupy liquid. Keep in well-stoppered
bottles.
XII.—Dissolve 3 parts of glue in small pieces in 12 to 15 of saccharate
of lime. By heating, the glue dissolves rapidly and remains liquid,
when cold, without loss of adhesive power. Any desirable consistence
can be secured by varying the amount of saccharate of lime. Thick
glue retains its muddy color, while a thin solution becomes clear on
standing.
The saccharate of lime is prepared by {12} dissolving 1 part of sugar
in 3 parts of water, and after adding 1/4 part of the weight of the
sugar of slaked lime, heating the whole from 149° to 185° F., allowing
it to macerate for several days, shaking it frequently. The solution,
which has the properties of mucilage, is then decanted from the
sediment.
XIII.—In a solution of borax in water soak a good quantity of glue
until it has thoroughly imbibed the liquid. Pour off the surplus
solution and then put on the water bath and melt the glue. Cool down
until the glue begins to set, then add, drop by drop, with agitation,
enough acetic acid to check the tendency to solidification. If, after
becoming quite cold, there is still a tendency to solidification, add a
few drops more of the acid. The liquid should be of the consistence of
ordinary mucilage at all times.
XIV.—Gelatin 100 parts
Cabinetmakers’ glue 100 parts
Alcohol 25 parts
Alum 2 parts
Acetic acid, 20 per cent 800 parts
Soak the gelatin and glue with the acetic acid and heat on a water bath
until fluid; then add the alum and alcohol.
XV.—Glue 10 parts
Water 15 parts
Sodium salicylate 1 part
XVI.—Soak 5 parts of Cologne glue in an aqueous calcium chloride
solution (1:4) and heat on the water bath until dissolved, replacing
the evaporating water; or slack 100 parts of lime with 150 parts of hot
water, dissolve 60 parts of sugar in 180 parts of water, and add 15
parts of the slacked lime to the solution, heating the whole to 75° C.
(167° F.). Place aside for a few days, shaking from time to time. In
the clear sugar-lime solution collected by decanting soak 60 parts of
glue and assist the solution by moderate heating.
XVII.—Molasses, 100 parts, dissolved in 300 parts of water, 25 parts
of quicklime (slaked to powder), being then stirred in and the
mixture heated to 167° F. on a water bath, with frequent stirrings.
After settling for a few days a large portion of the lime will have
dissolved, and the clear, white, thick solution, when decanted, behaves
like rubber solution and makes a highly adherent coating.
XVIII.—Dissolve bone glue, 250 parts, by heating in 1,000 parts of
water, and add to the solution barium peroxide 10 parts, sulphuric acid
(66° B.) 5 parts, and water 15 parts. Heat for 48 hours on the water
bath to 80° C. (176° F.). Thus a syrupy liquid is obtained, which is
allowed to settle and is then decanted. This glue has no unpleasant
odor, and does not mold.
XIX.—A glue possessing the adhesive qualities of ordinary joiners’
glue, but constituting a pale yellow liquid which is ready for use
without requiring heating and possesses great resistance to dampness,
is produced by treating dry casein with a diluted borax solution or
with enough ammonia solution to cause a faintly alkaline reaction. The
preparation may be employed alone or mixed with liquid starch in any
proportion.
«Glue for Celluloid.»—I.—Two parts shellac, 3 parts spirits of camphor,
and 4 parts strong alcohol dissolved in a warm place, give an excellent
gluing agent to fix wood, tin, and other bodies to celluloid. The glue
must be kept well corked up.
II.—A collodion solution may be used, or an alcoholic solution of fine
celluloid shavings.
«Glue to Form Paper Pads.»—
I.—Glue 3 1/2 ounces
Glycerine 8 ounces
Water, a sufficient quantity.
Pour upon the glue more than enough water to cover it and let stand for
several hours, then decant the greater portion of the water; apply heat
until the glue is dissolved, and add the glycerin. If the mixture is
too thick, add more water.
II.—Glue 6 ounces
Alum 30 grains
Acetic acid 1/2 ounce
Alcohol 1 1/2 ounces
Water 6 1/2 ounces
Mix all but the alcohol, digest on a water bath till the glue is
dissolved, allow to cool and add the alcohol.
III.—Glue 5 ounces
Water 1 ounce
Calcium chloride 1 ounce
Dissolve the calcium chloride in the water, add the glue, macerate
until it is thoroughly softened, and then heat until completely
dissolved.
IV.—Glue 20 ounces
Glycerine 5 ounces
Syrupy glucose 1 ounce
Tannin 50 grains
Cover the glue with cold water, and let stand over night. In the
morning pour off superfluous water, throw the glue on muslin, and
manipulate so as to get rid of as much moisture as possible, then put
in a water bath and melt. Add the {13} glycerine and syrup, and stir
well in. Finally, dissolve the tannin in the smallest quantity of water
possible and add.
This mixture must be used hot.
V.—Glue 15 ounces
Glycerine 5 ounces
Linseed oil 2 ounces
Sugar 1 ounce
Soak the glue as before, melt, add the sugar and glycerine, continuing
the heat, and finally add the oil gradually under constant stirring.
This must be used hot.
«Glue for Tablets.»—
I.—Glue 3 1/2 ounces
Glycerine 8 ounces
Water, a sufficient quantity.
Pour upon the glue more than enough water to cover it and let stand for
several hours, then decant the greater portion of the water; apply heat
until the glue is dissolved, and add the glycerine. If the mixture is
too thick, add more water.
II.—Glue 6 ounces
Alum 30 grains
Acetic acid 1/2 ounce
Alcohol 1 1/2 ounces
Water 6 1/2 ounces
Mix all but the alcohol, digest on a water bath till the glue is
dissolved, allow to cool and add the alcohol.
III.—Glue 5 ounces
Water 1 ounce
Calcium chloride 1 ounce
Dissolve the calcium chloride in the water, add the glue, macerate
until it is thoroughly softened, and then apply heat until completely
dissolved.
IV.—Glue, 1 pound; glycerine, 4 ounces; glucose syrup, 2
tablespoonfuls; tannin, 1/10 ounce. Use warm, and give an hour to dry
and set on the pads. This can be colored with any aniline dye.
«Marine Glue.»—Marine glue is a product consisting of shellac and
caoutchouc, which is mixed differently according to the use for which
it is required. The quantity of benzol used as solvent governs the
hardness or softness of the glue.
I.—One part Pará caoutchouc is dissolved in 12 parts benzol; 20
parts powdered shellac are added to the solution, and the mixture is
carefully heated.
II.—Stronger glue is obtained by dissolving 10 parts good crude
caoutchouc in 120 parts benzine or naphtha which solution is poured
slowly and in a fine stream into 20 parts asphaltum melted in a kettle,
stirring constantly and heating. Pour the finished glue, after the
solvent has almost evaporated and the mass has become quite uniform,
into flat molds, in which it solidifies into very hard tablets of dark
brown or black color. For use, these glue tablets are first soaked in
boiling water and then heated over a free flame until the marine glue
has become thinly liquid. The pieces to be glued are also warmed and a
very durable union is obtained.
III.—Cut caoutchouc into small pieces and dissolve in coal naphtha by
heat and agitation. Add to this solution powdered shellac, and heat
the whole, constantly stirring until combination takes place, then pour
it on metal plates to form sheets. When used it must be heated to 248°
F., and applied with a brush.
«Water-Proof Glues.»—I.—The glue is put in water till it is soft, and
subsequently melted in linseed oil at moderate heat. This glue is
affected neither by water nor by vapors.
II.—Dissolve a small quantity of sandarac and mastic in a little
alcohol, and add a little turpentine. The solution is boiled in a
kettle over the fire, and an equal quantity of a strong hot solution of
glue and isinglass is added. Then filter through a cloth while hot.
III.—Water-proof glue may also be produced by the simple addition of
bichromate of potassium to the liquid glue solution, and subsequent
exposure to the air.
IV.—Mix glue as usual, and then add linseed oil in the proportion of
1 part oil to 8 parts glue. If it is desired that the mixture remain
liquid, 1/2 ounce of nitric acid should be added to every pound of
glue. This will also prevent the glue from souring.
V.—In 1,000 parts of rectified alcohol dissolve 60 parts of sandarac
and as much mastic whereupon add 60 parts of white oil of turpentine.
Next, prepare a rather strong glue solution and add about the like
quantity of isinglass, heating the solution until it commences to boil;
then slowly add the hot glue solution till a thin paste forms, which
can still be filtered through a cloth. Heat the solution before use and
employ like ordinary glue. A connection effected with this glue is not
dissolved by cold water and even resists hot water for a long time.
VI.—Soak 1,000 parts of Cologne glue in cold water for 12 hours and in
another vessel for the same length of time 150 parts of isinglass in a
mixture of lamp spirit and water. Then dissolve both masses together on
the water bath in a suitable vessel, thinning, if necessary, with some
hot water. Next add 100 {14} parts of linseed oil varnish and filter
hot through linen.
VII.—Ordinary glue is kept in water until it swells up without losing
its shape. Thus softened it is placed in an iron crucible without
adding water; then add linseed oil according to the quantity of the
glue and leave this mixture to boil over a slow fire until a gelatinous
mass results. Such glue unites materials in a very durable manner. It
adheres firmly and hardens quickly. Its chief advantage, however,
consists in that it neither absorbs water nor allows it to pass
through, whereby the connecting places are often destroyed. A little
borax will prevent putrefaction.
VIII.—Bichromate of potassium 40 parts (by weight); gelatin glue, 55
parts; alum, 5 parts. Dissolve the glue in a little water and add the
bichromate of potassium and the alum.
IX.—This preparation permits an absolutely permanent gluing of pieces
of cardboard, even when they are moistened by water. Melt together
equal parts of good pitch and gutta-percha; of this take 9 parts, and
add to it 3 parts of boiled linseed oil and 1 1/2 parts of litharge.
Place this over the fire and stir it till all the ingredients are
intimately mixed. The mixture may be diluted with a little benzine or
oil of turpentine, and must be warm when used.
«Glue to Fasten Linoleum on Iron Stairs.»—I.—Use a mixture of glue,
isinglass, and dextrin which, dissolved in water and heated, is given
an admixture of turpentine. The strips pasted down must be weighted
with boards and brick on top until the adhesive agent has hardened.
II.—Soak 3 parts of glue in 8 parts water, add 1/2 part hydrochloric
acid and 3/4 part zinc vitriol and let this mixture boil several
hours. Coat the floor and the back of the linoleum with this. Press the
linoleum down uniformly and firmly and weight it for some time.
«Glue for Attaching Gloss to Precious Metals.»—Sandarac varnish, 15
parts; marine glue, 5 parts; drying oil, 5 parts; white lead, 5 parts;
Spanish white, 5 parts; turpentine, 5 parts. Triturate all to form a
rather homogeneous paste. This glue becomes very hard and resisting.
«Elastic Glue.»—Although elastic glue is less durable than rubber,
and will not stand much heat, yet it is cheaper than rubber, and is
not, like rubber affected by oil colors. Hence it is largely used for
printing rollers and stamps. For stamps, good glue is soaked for 24
hours in soft water. The water is poured off, and the swollen glue is
melted and mixed with glycerine and a little salicylic acid and cast
into molds. The durability is increased by painting the mass with a
solution of tannin, or, better, of bichromate of potassium. Printing
rollers require greater firmness and elasticity. The mass for them
once consisted solely of glue and vinegar, and their manufacture was
very difficult. The use of glycerine has remedied this, and gives
great elasticity without adhesiveness, and has removed the liability
of moldiness. Swollen glue, which has been superficially dried, is
fused with glycerine and cast into oil molds. Similar mixtures are
used for casting plaster ornaments, etc., and give very sharp casts.
A mass consisting of glue and glycerine is poured over the model in a
box. When the mold is removed, it is painted with plaster outside and
with boiled oil inside, and can then be used many times for making
reproductions of the model.
«Glue for Paper and Metal.»—A glue which will keep well and adhere
tightly is obtained by diluting 1,000 parts by weight of potato starch
in 1,200 parts by weight of water and adding 50 parts by weight of
pure nitric acid. The mixture is kept in a hot place for 48 hours,
taking care to stir frequently. It is afterwards boiled to a thick and
transparent consistency, diluted with water if there is occasion, and
then there are added in the form of a screened powder, 2 parts of sal
ammoniac and 1 part of sulphur flowers.
«Glue for Attaching Cloth Strips to Iron.»—Soak 500 parts of Cologne
glue in the evening with clean cold water in a clean vessel; in the
morning pour off the water, place the softened glue without admixture
of water into a clean copper or enamel receptacle, which is put on a
moderate low fire (charcoal or steam apparatus). During the dissolution
the mass must be continually stirred with a wooden trowel or spatula.
If the glue is too thick, it is thinned with diluted spirit, but not
with water. As soon as the glue has reached the boiling point, about
50 parts of linseed oil varnish (boiled oil) is added to the mass with
constant stirring. When the latter has been stirred up well, add 50
parts of powdered colophony and shake it into the mass with stirring,
subsequently removing the glue from the fire. In order to increase the
binding qualities and to guard against moisture, it is well still to
add about 50 parts of isinglass, which has been previously cut {15}
into narrow strips and placed, well beaten, in a vessel, into which
enough spirit of wine has been poured to cover all. When dissolved, the
last-named mass is added to the boiling glue with constant stirring.
The adhesive agent is now ready for use and is employed hot, it
being advisable to warm the iron also. Apply glue only to a surface
equivalent to a single strip at a time. The strips are pressed down
with a stiff brush or a wad of cloth.
«Glue for Leather or Cardboard.»—To attach leather to cardboard
dissolve good glue (softened by spelling in water) with a little
turpentine and enough water in an ordinary glue pot, and then having
made a thick paste with starch in the proportion of 2 parts by weight,
of starch powder for every 1 part, by weight, of dry glue, mix the
compounds and allow the mixture to become cold before application to
the cardboard.
«For Wood, Glass, Cardboard, and all Articles of a Metallic or Mineral
Character.»—Take boiled linseed oil 20 parts, Flemish glue 20 parts,
hydrated lime 15 parts, powdered turpentine 5 parts, alum 5 parts
acetic acid 5 parts. Dissolve the glue with the acetic acid, add the
alum, then the hydrated lime, and finally the turpentine and the boiled
linseed oil. Triturate all well until it forms a homogeneous paste and
keep in well-closed flasks. Use like any other glue.
«Glue for Uniting Metals with Fabrics.»—Cologne glue of good quality
is soaked and boiled down to the consistency of that used by
cabinetmakers. Then add, with constant stirring, sifted wood ashes
until a moderately thick, homogeneous mass results. Use hot and press
the pieces well together during the drying. For tinfoil, about 2 per
cent of boracic acid should be added instead of the wood ashes.
«Glue or Paste for Making Paper Boxes.»—
Chloral hydrate 5 parts
Gelatin, white 8 parts
Gum arabic 2 parts
Boiling water 30 parts
Mix the chloral, gelatin, and gum arabic in a porcelain container, pour
the boiling water over the mixture and let stand for 1 day, giving it
a vigorous stirring several times during the day. In cold weather this
is apt to get hard and stiff, but this may be obviated by standing the
container in warm water for a few minutes. This paste adheres to any
surface whatever.
«Natural Glue for Cementing Porcelain, Crystal Glass, etc.»—The large
shell snails which are found in vineyards have at the extremity of
their body a small, whitish bladder filled with a substance of greasy
and gelatinous aspect. If this substance extracted from the bladder
is applied on the fragments of porcelain or any body whatever, which
are juxtaposed by being made to touch at all parts, they acquire such
adhesion that if one strives to separate them by a blow, they are
more liable to break at another place than the cemented seam. It is
necessary to give this glue sufficient time to dry perfectly, so as to
permit it to acquire the highest degree of strength and tenacity.
«Belt Glue.»—A glue for belts can be prepared as follows: Soak 50
parts of gelatin in water, pour off the excess of water, and heat on
the water bath. With good stirring add, first, 5 parts, by weight, of
glycerine, then 10 parts, by weight, of turpentine, and 5 parts, by
weight, of linseed oil varnish and thin with water as required. The
ends of the belts to be glued are cut off obliquely and warmed; then
the hot glue is applied, and the united parts are subjected to strong
pressure, allowing them to dry thus for 24 hours before the belts are
used.
«Chromium Glue for Wood, Paper, and Cloth.»—I.—(_a_) One-half pound
strong glue (any glue if color is immaterial, white fish glue
otherwise); soak 12 hours in 12 fluidounces of cold water. (_b_)
One-quarter pound gelatin; soak 2 hours in 12 fluidounces cold water.
(_c_) Two ounces bichromate of potassium dissolved in 8 fluidounces
boiling water. Dissolve (_a_) after soaking, in a glue pot, and add
(_b_). After (_a_) and (_b_) are mixed and dissolved, stir in (_c_).
This glue is exceedingly strong, and if the article cemented be exposed
to strong sunlight for 1 hour, the glue becomes perfectly waterproof.
Of course, it is understood that the exposure to sunlight is to be made
after the glue is thoroughly dry. The one objectionable feature of this
cement is its color, which is a yellow-brown. By substituting chrome
alum in place of the bichromate, an olive color is obtained.
II.—Use a moderately strong gelatin solution (containing 5 to 10
per cent of dry gelatin), to which about 1 part of acid chromate of
potassium in solution is added to every 5 parts of gelatin. This
mixture has the property of becoming insoluble by water through the
action of sunlight under partial reduction of the chromic acid. {16}
«Fireproof Glue.»—
Raw linseed oil 8 parts
Glue or gelatin 1 part
Quicklime 2 parts
Soak the glue or gelatin in the oil for 10 to 12 hours, and then melt
it by gently heating the oil, and when perfectly fluid stir in the
quicklime until the whole mass is homogeneous, then spread out in
layers to dry gradually, out of the sun’s rays. For use, reheat the
glue in a glue pot in the ordinary way of melting glue.
«CEMENTS.»
Under this heading will be found only cements for causing one substance
to adhere to another. Cements used primarily as fillers, such as dental
cements, will be found under Cements, Putties, etc.
«Cutlers’ Cements for Fixing Knife Blades into Handles.»—
I.—Rosin 4 pounds
Beeswax 1 pound
Plaster of Paris or brickdust 1 pound
II.—Pitch 5 pounds
Wood ashes 1 pound
Tallow 1 pound
III.—Rosin, 12; sulphur flowers, 3; iron filings, 5. Melt together,
fill the handle while hot, and insert the instrument.
IV.—Plaster of Paris is ordinarily used for fastening loose handles.
It is made into a moderately thick paste with water run into the hole
in the head of the pestle, the handle inserted and held in place till
the cement hardens. Some add sand to the paste, and claim to get better
results.
V.—Boil together 1 part of caustic soda, 3 parts of rosin, and 5 parts
of water till homogeneous and add 4 parts of plaster of Paris. The
paste sets in half an hour and is but little affected by water.
VI.—Equal quantities of gutta percha and shellac are melted together
and well stirred. This is best done in an iron capsule placed on a
sandbath and heated over a gas furnace or on the top of a stove. The
combination possesses both hardness and toughness, qualities that make
it particularly desirable in mending mortars and pestles. In using, the
articles to be cemented should be warmed to about the melting point of
the mixture and retained in proper position until cool, when they are
ready for use.
VII.—Rosin 600 parts by weight
Sulphur 150 parts by weight
Iron filings 250 parts by weight
Pour the mixture, hot, into the opening of the heated handle and shove
in the knife likewise heated.
VIII.—Melt sufficient black rosin, and incorporate thoroughly with it
one-fifth its weight of very fine silver sand. Make the pestle hot,
pour in a little of the mixture, then force the handle well home, and
set aside for a day before using.
IX.—Make a smooth, moderately soft paste with litharge and glycerine;
fill the hole in the pestle with the cement, and firmly press the
handle in place, keeping it under pressure for three or four days.
«Cements for Stone.»—I.—An excellent cement for broken marble consists
of 4 parts of gypsum and 1 part of finely powdered gum arabic. Mix
intimately. Then with a cold solution of borax make into a mortarlike
mass. Smear on each face of the parts to be joined, and fasten the bits
of marble together. In the course of a few days the cement becomes
very hard and holds very tenaciously. The object mended should not be
touched for several days. In mending colored marbles the cement may be
given the hue of the marble by adding the color to the borax solution.
II.—A cement which dries instantaneously, qualifying it for all sorts
of repairing and only presenting the disadvantage of having to be
freshly prepared each time, notwithstanding any subsequent heating, may
be made as follows: In a metal vessel or iron spoon melt 4 to 5 parts
of rosin (or preferably mastic) and 1 part of beeswax. This mixture
must be applied rapidly, it being of advantage slightly to heat the
surfaces to be united, which naturally must have been previously well
cleaned.
III.—Slaked lime, 10 parts; chalk, 15 parts; kaolin, 5 parts; mix, and
immediately before use stir with a corresponding amount of potash water
glass.
IV.—Cement on Marble Slabs.—The whole marble slab is thoroughly warmed
and laid face down upon a neatly cleaned planing bench upon which a
woolen cloth is spread so as not to injure the polish of the slab. Next
apply to the slab very hot, weak glue and quickly sift hot plaster of
Paris on the glue in a thin even layer, stirring the plaster rapidly
into the applied glue by means of a strong spatula, so that a uniform
glue-plaster coating is formed on the warm slab. Before this has time
to harden tip the respective piece of furniture on the slab. The frame,
likewise warmed, will adhere very firmly to the slab after two days.
Besides, this process has the advantage of great cleanliness. {17}
V.—The following is a recipe used by marble workers, and which probably
can be used to advantage: Flour of sulphur, 1 part; hydrochlorate of
ammonia, 2 parts; iron filings, 16 parts. The above substances must
be reduced to a powder, and securely preserved in closely stoppered
vessels. When the cement is to be employed, take 20 parts very fine
iron filings and 1 part of the above powder; mix them together with
enough water to form a manageable paste. This paste solidifies in 20
days and becomes as hard as iron. A recipe for another cement useful
for joining small pieces of marble or alabaster is as follows: Add
1/2 pint of vinegar to 1/2 pint skimmed milk; mix the curd with the
whites of 5 eggs, well beaten, and sufficient powdered quicklime sifted
in with constant stirring so as to form a paste. It resists water and a
moderate degree of heat.
VI.—Cement for Iron and Marble.—For fastening iron to marble or stone a
good cement is made as follows: Thirty parts plaster of Paris, 10 parts
iron filings, 1/2 part sal ammoniac mixed with vinegar to a fluid
paste fresh for use.
«Cement for Sandstones.»—One part sulphur and 1 part rosin are melted
separately; the melted masses are mixed and 3 parts litharge and 2
parts ground glass stirred in. The latter ingredients must be perfectly
dry, and have been well pulverized and mixed previously.
Equally good cement is obtained by melting together 1 part pitch and
1/10 part wax, and mixing with 2 parts brickdust.
The stones to be cemented, or between the joints of which the putty
is to be poured, must be perfectly dry. If practicable, they should
be warmed a little, and the surfaces to which the putty is to adhere
painted with oil varnish once or twice. The above two formulæ are of
especial value in case the stones are very much exposed to the heat
of the sun in summer, as well as to cold, rain, and snow in winter.
Experience has shown that in these instances the above-mentioned
cements give better satisfaction than the other brands of cement.
«Cements for Attaching Objects to Glass.»—
Rosin 1 part
Yellow wax 2 parts
Melt together.
«To Attach Copper to Glass.»—Boil 1 part of caustic soda and 3 parts of
colophony in 5 parts of water and mix with the like quantity of plaster
of Paris. This cement is not attacked by water, heat, and petroleum.
If, in place of the plaster of Paris, zinc white, white lead, or slaked
lime is used, the cement hardens more slowly.
«To Fasten Brass upon Glass.»—Boil together 1 part of caustic soda, 3
parts of rosin, 3 parts of gypsum, and 5 parts of water. The cement
made in this way hardens in about half an hour, hence it must
be applied quickly. During the preparation it should be stirred
constantly. All the ingredients used must be in a finely powdered state.
«Uniting Glass with Horn.»—(1) A solution of 2 parts of gelatin in
20 parts water is evaporated up to one-sixth of its volume and 1/3
mastic dissolved in 1/2 spirit added and some zinc white stirred in.
The putty is applied warm; it dries easily and can be kept a long time.
(2) Mix gold size with the equal volume of water glass.
«To Cement Glass to Iron.»—
I.—Rosin 5 ounces
Yellow wax 1 ounce
Venetian red 1 ounce
Melt the wax and rosin on a water bath and add, under constant
stirring, the Venetian red previously well dried. Stir until nearly
cool, so as to prevent the Venetian red from settling to the bottom.
II.—Portland cement 2 ounces
Prepared chalk 1 ounce
Fine sand 1 ounce
Solution of sodium silicate
enough to form a semi-liquid
paste.
III.—Litharge 2 parts
White lead 1 part
Work into a pasty condition by using 3 parts boiled linseed oil, 1 part
copal varnish.
«Celluloid Cements.»—I.—To mend broken draughting triangles and other
celluloid articles, use 3 parts alcohol and 4 parts ether mixed
together and applied to the fracture with a brush until the edges
become warm. The edges are then stuck together, and left to dry for at
least 24 hours.
II.—Camphor, 1 part; alcohol, 4 parts. Dissolve and add equal quantity
(by weight) of shellac to this solution.
III.—If firmness is desired in putting celluloid on wood, tin, etc.,
the following gluing agent is recommended, viz.: A compound of 2 parts
shellac, 3 parts spirit of camphor, and 4 parts strong alcohol. {18}
IV.—Shellac 2 ounces
Spirits of camphor 2 ounces
Alcohol, 90 per cent 6 to 8 ounces
V.—Make a moderately strong glue or solution of gelatin. In a dark
place or a dark room mix with the above a small amount of concentrated
solution of potassium dichromate. Coat the back of the label, which
must be clean, with a thin layer of the mixture. Strongly press the
label against the bottle and keep the two in close contact by tying
with twine or otherwise. Expose to sunlight for some hours; this causes
the cement to be insoluble even in hot water.
VI.—Lime av. oz. 1
White of egg av. oz. 2 1/2
Plaster of Paris av. oz. 5 1/2
Water fl. oz. 1
Reduce the lime to a fine powder; mix it with the white of egg by
trituration, forming a uniform paste. Dilute with water, rapidly
incorporate the plaster of Paris, and use the cement immediately. The
surfaces to be cemented must first be moistened with water so that the
cement will readily adhere. The pieces must be firmly pressed together
and kept in this position for about 12 hours.
«Cementing Celluloid and Hard-Rubber Articles.»—I.—Celluloid articles
can be mended by making a mixture composed of 3 parts of alcohol and 4
parts of ether. This mixture should be kept in a well-corked bottle,
and when celluloid articles are to be mended, the broken surfaces are
painted over with the alcohol and ether mixture until the surfaces
soften: then press together and bind and allow to dry for at least 24
hours.
II.—Dissolve 1 part of gum camphor in 4 parts of alcohol; dissolve an
equal weight of shellac in such strong camphor solution. The cement
is applied warm and the parts united must not be disturbed until the
cement is hard. Hard-rubber articles are never mended to form a strong
joint.
III.—Melt together equal parts of gutta percha and real asphaltum. The
cement is applied hot, and the broken surfaces pressed together and
held in place while cooling.
«Sign-Letter Cements.»—
I.—Copal varnish 15 parts
Drying oil 5 parts
Turpentine (spirits) 3 parts
Oil of turpentine 2 parts
Liquefied glue 5 parts
Melt all together on a water bath until well mixed, and then add 10
parts slaked lime.
II.—Mix 100 parts finely powdered white litharge with 50 parts dry
white lead, knead together 3 parts linseed oil varnish and 1 part copal
varnish into a firm dough. Coat the side to be attached with this,
removing the superfluous cement. It will dry quickly and become very
hard.
III.—Copal varnish 15 parts
Linseed-oil varnish 5 parts
Raw turpentine 3 parts
Oil of turpentine 2 parts
Carpenters’ glue, dissolved in water 5 parts
Precipitated chalk 10 parts
IV.—Mastic gum 1 part
Litharge, lead 2 parts
White lead 1 part
Linseed oil 3 parts
Melt together to a homogeneous mass. Apply hot. To make a thorough and
reliable job, the letters should be heated to at least the temperature
of the cement.
«To Fix Gold Letters, etc., upon Glass.»—I.—The glass must be entirely
clean and polished, and the medium is prepared in the following manner:
One ounce fish glue or isinglass is dissolved in water so that the
latter covers the glue. When this is dissolved a quart of rectified
spirit of wine is added, and enough water is poured in to make up
one-quarter the whole. The substance must be kept well corked.
II.—Take 1/2 quart of the best rum and 1/4 ounce fish glue, which
is dissolved in the former at a moderate degree of heat. Then add 1/2
quart distilled water, and filter through a piece of old linen. The
glass is laid upon a perfectly level table and is covered with this
substance to the thickness of 1/8 inch, using a clean brush. Seize
the gold leaf with a pointed object and place it smoothly upon the
prepared mass, and it will be attracted by the glass at once. After 5
minutes hold the glass slightly slanting so that the superfluous mass
can run off, and leave the plate in this position for 24 hours, when
it will be perfectly dry. Now trace the letters or the design on a
piece of paper, and perforate the lines with a thick needle, making
the holes 1/16 inch apart. Then place the perforated paper upon the
surface of the glass, and stamp the tracery on with powdered chalk.
The paper pattern is then carefully removed, and the accurate design
will remain upon the gold. The outlines are now filled out with an oily
gold mass, mixed with a little chrome orange and diluted with boiled
oil or turpentine. When all is dry the superfluous gold is washed off
{19} with water by means of a common rag. The back of the glass is then
painted with a suitable color.
«Attaching Enamel Letters to Glass.»—To affix enamel letters to glass,
first clean the surface of the glass perfectly, leaving no grease or
sticky substance of any kind adhering to the surface. Then with a piece
of soap sketch the outlines of the design. Make the proper division
of the guide lines, and strike off accurately the position each letter
is to occupy. Then to the back of the letters apply a cement made as
follows: White lead ground in oil, 2 parts; dry white lead, 3 parts.
Mix to a soft putty consistency with good copal varnish.
With a small knife or spatula apply the cement to the back of the
letters, observing especial care in getting the mixture well and
uniformly laid around the inside edges of the letter. In attaching
the letters to the glass make sure to expel the air from beneath the
characters, and to do this, work them up and down and sidewise. If the
weather be at all warm, support the letters while drying by pressing
tiny beads of sealing wax against the glass, close to the under side
or bottom of the letters. With a putty knife, keenly sharpened on one
edge, next remove all the surplus cement. Give the letters a hard, firm
pressure against the glass around all edges to securely guard against
the disruptive attacks of moisture.
The seepage of moisture beneath the surface of the letters is the main
cause of their early detachment from the glass.
The removal of the letters from the glass may be effected by applying
turpentine to the top of the characters, allowing it to soak down and
through the cement. Oxalic acid applied in the same way will usually
slick the letters off in a trice.
«Cement for Porcelain Letters.»—Slake 15 parts of fresh quicklime in 20
parts of water. Melt 50 parts of caoutchouc and 50 parts of linseed-oil
varnish together, and bring the mixture to a boil. While boiling,
pour the liquid on the slaked lime, little by little, under constant
stirring. Pass the mixture, while still hot, through muslin, to remove
any possible lumps, and let cool. It takes the cement 2 days to set
completely, but when dry it makes a joint that will resist a great
deal of strain. By thinning the mixture down with oil of turpentine, a
brilliant, powerfully adhesive varnish is obtained.
«Water-Glass Cements.»—I.—Water glass (sodium of potassium silicate),
which is frequently recommended for cementing glass, does not, as is
often asserted, form a vitreous connection between the joined surfaces;
and, in fact, some of the commercial varieties will not even dry, but
merely form a thick paste, which has a strong affinity for moisture.
Good 30° B. water glass is, however, suitable for mending articles that
are exposed to heat, and is best applied to surfaces that have been
gently warmed; when the pieces are put together they should be pressed
warmly, to expel any superfluous cement, and then heated strongly.
To repair cracked glasses or bottles through which water will leak,
water glasses may be used, the application being effected in the
following easy manner: The vessel is warmed to induce rarefaction of
the internal air, after which the mouth is closed, either by a cork
in the case of bottles, or by a piece of parchment or bladder if a
wide-mouthed vessel is under treatment.
While still hot, the outside of the crack is covered with a little
glass, and the vessel set aside to cool, whereupon the difference
between the pressure of the external and internal air will force the
cement into the fissure and close it completely. All that is then
necessary is to take off the cover and leave the vessel to warm for a
few hours. Subsequently rinse it out with lime water, followed by clean
water, and it will then hold any liquid, acids and alkaline fluids
alone excepted.
II.—When water glass is brought into contact with calcium chloride,
a calcium silicate is at once formed which is insoluble in water. It
seems possible that this reaction may be used in binding together
masses of sand, etc. The process indicated has long been used in the
preservation of stone which has become “weathered.” The stone is first
brushed with the water glass and afterwards with a solution of calcium
chloride. The conditions here are of course different.
Calcium chloride must not be confounded with the so-called “chloride of
lime” which is a mixture of calcium hypochlorite and other bodies.
«To Fasten Paper Tickets to Glass.»—To attach paper tickets to glass,
the employment of water glass is efficacious. Care should be taken
to spread this product on the glass and not on the paper, and then
to apply the paper dry, which should be done immediately. When the
solution is dry the paper cannot be {20} detached. The silicate should
be somewhat diluted. It is spread on the glass with a rag or a small
sponge.
«JEWELERS’ CEMENTS.»
Jewelers and goldsmiths require, for the cementing of genuine and
colored gems, as well as for the placing of colored folio under
certain stones, very adhesive gluing agents, which must, however,
be colorless. In this respect these are distinguished chiefly by the
so-called diamond cement and the regular jewelers’ cement. Diamond
cement is much esteemed by jewelers for cementing precious stones and
corals, but may also be employed with advantage for laying colored
fluxes of glass on white glass. The diamond cement is of such a nature
as to be able to remain for some time in contact with water without
becoming soft. It adheres best between glass or between precious
stones. It is composed as follows: Isinglass 8 parts, gum ammoniac 1
part, galbanum 1 part, spirit of wine 4 parts. Soak the isinglass in
water with admixture of a little spirit of wine and add the solution
of the gums in the remainder of the spirit of wine. Before use, heat
the diamond cement a little so as to soften it. Jewelers’ cement is
used for similar purposes as is the diamond cement, and is prepared
from: Isinglass (dry) 10 parts, mastic varnish 5 parts. Dissolve the
isinglass in very little water, adding some strong spirit of wine. The
mastic varnish is prepared by pouring a mixture of highly rectified
spirit of wine and benzine over finely powdered mastic and dissolving
it in the smallest possible quantity of liquid. The two solutions of
isinglass and mastic are intimately ground together in a porcelain dish.
«Armenian Cement.»—The celebrated “Armenian” cement, so called formerly
used by Turkish and Oriental jewelers generally, for setting precious
stones, “facing diamonds,” rubies, etc., is made as follows:
Mastic gum 10 parts
Isinglass (fish glue) 20 parts
Gum ammoniac 5 parts
Alcohol absolute 60 parts
Alcohol, 50 per cent 35 parts
Water 100 parts
Dissolve the mastic in the absolute alcohol; dissolve, by the aid of
gentle heat, on the water bath, the isinglass in the water, and add 10
parts of the dilute alcohol. Now dissolve the ammoniacum in the residue
of the dilute alcohol. Add the first solution to the second, mix
thoroughly by agitation and then add the solution of gum ammoniac and
stir well in. Finally put on the water bath, and keeping at a moderate
heat, evaporate the whole down to 175 parts.
«Cement for Enameled Dials.»—The following is a good cement for
enameled dials, plates, or other pieces: Grind into a fine powder
2 1/2 parts of dammar rosin and 2 1/2 parts of copal, using
colorless pieces if possible. Next add 2 parts of Venetian turpentine
and enough spirit of wine so that the whole forms a thick paste. To
this grind 3 parts of the finest zinc white. The mass now has the
consistency of prepared oil paint. To remove the yellow tinge of the
cement add a trifle of Berlin blue to the zinc white. Finally, the
whole is heated until the spirit of wine is driven off and a molten
mass remains, which is allowed to cool and is kept for use. Heat the
parts to be cemented.
«Watch-Lid Cement.»—The hardest cement for fixing on watch lids is
shellac. If the lids are exceedingly thin the engraving will always
press through. Before cementing it on the inside of the lid, in order
not to injure the polish, it is coated with chalk dissolved in alcohol,
which is first allowed to dry. Next melt the shellac on the stick, heat
the watch lid and put it on. After the engraving has been done, simply
force the lid off and remove the remaining shellac from the latter by
light tapping. If this does not remove it completely lay the lid in
alcohol, leaving it therein until all the shellac has dissolved. All
that remains to be done now is to wash out the watch lid.
«Jewelers’ Glue Cement.»—Dissolve on a water bath 50 parts of fish glue
in a little 95-per-cent alcohol, adding 4 parts, by weight, of gum
ammoniac. On the other hand, dissolve 2 parts, by weight, of mastic in
10 parts, by weight, of alcohol. Mix these two solutions and preserve
in a well-corked flask. For use it suffices to soften it on the water
bath.
«Casein Cements.»—
I.—Borax 5 parts
Water 95 parts
Casein, sufficient quantity.
Dissolve the borax in water and incorporate enough casein to produce a
mass of the proper consistency.
II.—The casein is made feebly alkaline by means of soda or potash lye
and {21} then subjected for about 24 hours to a temperature of 140° F.
Next follow the customary admixture, such as lime and water glass, and
finally, to accomplish a quicker resinification, substances containing
tannin are added. For tannic admixtures to the partially disintegrated
casein, slight quantities—about 1 per cent—of gallic acid, cutch, or
quercitannic acid are employed. The feebly alkaline casein cement
containing tannic acid is used in the well-known manner for the gluing
together of wood.
«For Metals.»—Make a paste with 16 ounces casein, 20 ounces slaked
lime, and 20 ounces of sand, in water.
«For Glass.»—I.—Dissolve casein in a concentrated solution of borax.
II.—Make a paste of casein and water glass.
«Pasteboard and Paper Cement.»—I.—Let pure glue swell in cold water;
pour and press off the excess; put on the water bath and melt. Paper
or other material cemented with this is then immediately, before the
cement dries, submitted to the action of formaldehyde and dried. The
cement resists the action of water, even hot.
II.—Melt together equal parts of good pitch and gutta percha. To 9
parts of this mass add 3 parts of boiled linseed oil and 1/5 part
litharge. The heat is kept up until, with constant stirring, an
intimate union of all the ingredients has taken place. The mixture is
diluted with a little benzine or oil of turpentine and applied while
still warm. The cement is waterproof.
III.—The _National Druggist_ says that experience with pasting or
cementing parchment paper seems to show that about the best agent
is casein cement, made by dissolving casein in a saturated aqueous
solution of borax.
IV.—The following is recommended for paper boxes:
Chloral hydrate 5 parts
Gelatin, white 8 parts
Gum arabic 2 parts
Boiling water 30 parts
Mix the chloral, gelatin, and gum arabic in a porcelain container, pour
the boiling water over the mixture and let stand for 1 day, giving it
a vigorous stirring several times during the day. In cold weather this
is apt to get hard and stiff, but this may be obviated by standing the
container in warm water for a few minutes. This paste adheres to any
surface whatever.
«Waterproof Cements for Glass, Stoneware, and Metal.»—I.—Make a paste
of sulphur, sal ammoniac, iron filings, and boiled oil.
II.—Mix together dry: Whiting, 6 pounds; plaster of Paris, 3 pounds;
sand, 3 pounds; litharge, 3 pounds; rosin, 1 pound. Make to a paste
with copal varnish.
III.—Make a paste of boiled oil, 6 pounds; copal, 6 pounds; litharge, 2
pounds; white lead, 1 pound.
IV.—Make a paste with boiled oil, 3 pounds; brickdust 2 pounds; dry
slaked lime, 1 pound.
V.—Dissolve 93 ounces of alum and 93 ounces of sugar of lead in water
to concentration. Dissolve separately 152 ounces of gum arabic in 25
gallons of water, and then stir in 62 1/2 pounds of flour. Then heat
to a uniform paste with the metallic salts, but take care not to boil
the mass.
VI.—For Iron and Marble to Stand in Heat.—In 3 pounds of water dissolve
first, 1 pound water glass and then 1 pound of borax. With the solution
make 2 pounds of clay and 1 pound of barytes, first mixed dry, to a
paste.
VII.—Glue to Resist Boiling Water.—Dissolve separately in water 55
pounds of glue and a mixture of 40 pounds of bichromate and 5 pounds of
alum. Mix as wanted.
VIII. (Chinese Glue).—Dissolve shellac in 10 times its weight of
ammonia.
IX.—Make a paste of 40 ounces of dry slaked lime 10 ounces of alum, and
50 ounces of white of egg.
X.—Alcohol 1,000 parts
Sandarac 60 parts
Mastic 60 parts
Turpentine oil 60 parts
Dissolve the gums in the alcohol and add the oil and stir in. Now
prepare a solution of equal parts of glue and isinglass, by soaking 125
parts of each in cold water until it becomes saturated, pouring and
pressing off the residue, and melting on the water bath. This should
produce a volume of glue nearly equal to that of the solution of gums.
The latter should, in the meantime, have been cautiously raised to
the boiling point on the water bath, and then mixed with the hot glue
solution.
It is said that articles united with this substance will stand the
strain of cold water for an unlimited time, and it takes hot water even
a long time to affect it. {22}
XI.—Burgundy pitch 6 parts
Gutta percha 1 part
Pumice stone, in fine powder 3 parts
Melt the gutta percha very carefully add the pumice stone, and lastly
the pitch, and stir until homogeneous.
Use while still hot. This cement will withstand water and dilute
mineral acids.
«LEATHER AND RUBBER CEMENTS.»
I.—Use a melted mixture of gutta percha and genuine asphalt, applied
hot. The hard-rubber goods must be kept pressed together until the
cement has cooled.
II.—A cement which is effective for cementing rubber to iron and which
is especially valuable for fastening rubber bands to bandsaw wheels is
made as follows: Powdered shellac, 1 part; strong water of ammonia,
10 parts. Put the shellac in the ammonia water and set it away in a
tightly closed jar for 3 or 4 weeks. By that time the mixture will
become a perfectly liquid transparent mass and is then ready for
use. When applied to rubber the ammonia softens it, but it quickly
evaporates, leaving the rubber in the same condition as before. The
shellac clings to the iron and thus forms a firm bond between the iron
and the rubber.
III.—Gutta percha white 1 drachm
Carbon disulphide 1 ounce
Dissolve, filter, and add:
India rubber 15 grains
Dissolve.
«Cement for Metal on Hard Rubber.»—I.—Soak good Cologne glue and boil
down so as to give it the consistency of joiners’ glue, and add with
constant stirring, enough sifted wood ashes until a homogeneous,
moderately thick mass results. Use warm and fit the pieces well
together while drying.
«How to Unite Rubber and Leather.»—II.—Roughen both surfaces, the
leather and the rubber, with a sharp glass edge; apply to both a
diluted solution of gutta percha in carbon bisulphide and let this
solution soak into the material. Then press upon each surface a skin
of gutta percha 1/10 of an inch in thickness between rolls. The two
surfaces are now united in a press, which should be warm but not hot.
This method should answer in all cases in which it is applicable. The
other prescription covers cases in which a press cannot be used. Cut
30 parts of rubber into small pieces, and dissolve it in 140 parts of
carbon bisulphide, the vessel being placed on a water bath of 30° C.
(86° F.). Further, melt 10 parts of rubber with 15 of colophony, and
add 35 parts of oil of turpentine. When the rubber has been completely
dissolved, the two liquids may be mixed. The resulting cement must be
kept well corked.
«To Fasten Rubber to Wood.»—I.—Make a cement by macerating virgin gum
rubber, or as pure rubber as can be had, cut in small pieces, in just
enough naphtha or gasoline to cover it. Let it stand in a very tightly
corked or sealed jar for 14 days, or a sufficient time to become
dissolved, shaking the mixture daily.
II.—Dissolve pulverized gum shellac, 1 ounce, in 9 1/2 ounces of
strong ammonia. This of course must be kept tightly corked. It will not
be as elastic as the first preparation.
III.—Fuse together shellac and gutta percha in equal weights.
IV.—India rubber 8 ounces
Gutta percha 4 ounces
Isinglass 2 ounces
Bisulphide of carbon 32 ounces
V.—India rubber 5 ounces
Gum mastic 1 ounce
Chloroform 3 ounces
VI.—Gutta percha 16 ounces
India rubber 4 ounces
Pitch 4 ounces
Shellac 1 ounce
Linseed oil 1 ounce
Amalgamate by heat.
VII.—Mix 1 ounce of oil of turpentine with 10 ounces of bisulphide of
carbon in which as much gutta percha as possible has been dissolved.
VIII.—Amalgamate by heat:
Gutta percha 100 ounces
Venice turpentine 80 ounces
Shellac 8 ounces
India rubber 2 ounces
Liquid storax 10 ounces
IX.—Amalgamate by heat:
India rubber 100 ounces
Rosin 15 ounces
Shellac 10 ounces
Then dissolve in bisulphide of carbon.
X.—Make the following solutions separately and mix:
(_a_) India rubber 5 ounces
Chloroform 140 ounces
(_b_) India rubber 5 ounces
Rosin 2 ounces
Venice turpentine 1 ounce
Oil of turpentine 20 ounces
{23}
«Cement for Patching Rubber Boots and Shoes.»—
I.—India rubber, finely chopped 100 parts
Rosin 15 parts
Shellac 10 parts
Carbon disulphide, q. s. to dissolve.
This will not only unite leather to leather, india rubber, etc., but
will unite rubber to almost any substance.
II.—Caoutchouc, finely cut 4 parts
India rubber, finely cut 1 part
Carbon disulphide 32 parts
Dissolve the caoutchouc in the carbon disulphide, add the rubber, let
macerate a few days, then mash with a palette knife to a smooth paste.
The vessel in which the solution is made in both instances above must
be kept tightly closed, and should have frequent agitations.
III.—Take 100 parts of crude rubber or caoutchouc, cut it up in small
bits, and dissolve it in sufficient carbon bisulphide, add to it 15
parts of rosin and 10 parts of gum lac. The user must not overlook the
great inflammability and exceedingly volatile nature of the carbon
bisulphide.
«Tire Cements.»—
I.—India rubber 15 grams
Chloroform 2 ounces
Mastic 1/2 ounce
Mix the india rubber and chloroform together, and when dissolved, the
mastic is added in powder. It is then allowed to stand a week or two
before using.
II.—The following is recommended as very good for cementing pneumatic
tires to bicycle wheels:
Shellac 1 ounce
Gutta percha 1 ounce
Sulphur 45 grains
Red lead 45 grains
Melt together the shellac and gutta percha, then add, with constant
stirring, the sulphur and red lead. Use while hot.
III.—Raw gutta percha 16 ounces
Carbon bisulphide 72 ounces
Eau de Cologne 2 2/3 ounces
This cement is the subject of an English patent and is recommended for
patching cycle and motor tires, insulating electric wires, etc.
IV.—A good thick shellac varnish with which a small amount of castor
oil has been mixed will be found a very excellent bicycle rim cement.
The formula recommended by Edel is as follows:
Shellac 1 pound
Alcohol 1 pint
Mix and dissolve, then add:
Castor oil 1/2 ounce
The castor oil prevents the cement from becoming hard and brittle.
A cement used to fasten bicycle tires may be made by melting together
at a gentle heat equal parts of gutta percha and asphalt. Apply hot.
Sometimes a small quantity each of sulphur and red lead is added (about
1 part of each to 20 parts of cement).
«Cements for Leather.»—
I.—Gutta percha 20 parts
Syrian asphalt, powdered 20 parts
Carbon disulphide 50 parts
Oil of turpentine 10 parts
The gutta percha, shredded fine, is dissolved in the carbon disulphide
and turpentine oil. To the solution add the asphalt and set away for
several days, or until the asphalt is dissolved. The cement should have
the consistency of honey. If the preparation is thinner than this let
it stand, open, for a few days. Articles to be patched should first be
washed with benzine.
II.—Glue 1 ounce
Starch paste 2 ounces
Turpentine 1 drachm
Water, a sufficient quantity.
Dissolve the glue in sufficient water with heat; mix the starch paste
with water; add the turpentine, and finally mix with the glue while hot.
III.—Soak for one day 1 pound of common glue in enough water to cover,
and 1 pound of isinglass in ale droppings. Then mix together and heat
gently until boiling. At this point add a little pure tannin and keep
boiling for an hour. If the glue and isinglass when mixed are too
thick, add water. This cement should be used warm and the jointed
leather pressed tightly together for 12 hours.
IV.—A waterproof cement for leather caoutchouc, or balata, is prepared
by dissolving gutta percha, caoutchouc, benzoin, gum lac, mastic,
etc., in some convenient solvent like carbon disulphide, chloroform,
ether, or alcohol. The best solvent, however, in the case of gutta
percha, is carbon disulphide and ether for mastic. The most favorable
proportions are as follows: Gutta percha, 200 to 300 parts to 100 parts
of the solvent, and 75 to 85 parts of mastic to 100 parts of ether.
From 5 to 8 parts of the former solution are mixed with 1 {24} part of
the latter, and the mixture is then boiled on the water bath, or in a
vessel fitted with a water jacket.
V.—Make a solution of 200 to 300 parts of caoutchouc, gutta percha,
india rubber, benzoin, or similar gum, in 1,000 parts of carbon
disulphide, chloroform, ether, or alcohol, and of this add 5 to 8 parts
to a solution of mastic (75 to 125 parts) in ether 100 parts, of equal
volume and boil together. Use hot water as the boiling agent, or boil
very cautiously on the water bath.
VI.—Forty parts of aluminum acetate, 10° B., 10 parts of glue, 10 parts
of rye flour. These materials are either to be simultaneously mixed and
boiled, or else the glue is to be dissolved in the aluminum acetate,
and the flour stirred into the solution. This is an excellent cement
for leather, and is used in so-called art work with leather, and with
leather articles which are made of several pieces. It is to be applied
warm.
«Rubber Cement for Cloth.»—The following formulas have been recommended:
I.—Caoutchouc, 5 parts; chloroform, 3 parts. Dissolve and add gum
mastic (powder) 1 part.
II.—Gutta percha, 16 parts; india rubber, 4 parts; pitch, 2 parts;
shellac, 1 part; linseed oil, 2 parts. Reduce the solids to small
pieces, melt together with the oil and mix well.
III.—The following cement for mending rubber shoes and tires will
answer similar purposes:
Caoutchouc in shavings 10 parts by weight
Rosin 4 parts by weight
Gum turpentine 40 parts by weight
Oil turpentine, enough.
Melt together first the caoutchouc and rosin, then add the gum
turpentine, and when all is liquefied, add enough of oil of turpentine
to preserve it liquid. A second solution is prepared by dissolving
together:
Caoutchouc 10 parts by weight
Chloroform 280 parts by weight
For use these two solutions are mixed. Wash the hole in the rubber shoe
over with the cement, then a piece of linen dipped in it is placed
over it; as soon as the linen adheres to the sole, the cement is then
applied as thickly as required.
«CEMENTS FOR METALS AND FOR ATTACHING VARIOUS SUBSTANCES TO METALS:»
«Cements for Iron.»—I.—To make a good cement for iron on iron, make a
thick paste, with water, of powdered iron, 60 parts; sal ammoniac, 2
parts, and sulphur flowers, 1 part. Use while fresh.
II.—Sulphur flowers, 6 parts; dry white lead 6 parts, and powdered
borax, 1 part. Mix by sifting and keep as a dry powder in a closed tin
box. To use, make into a thin paste with strong sulphuric acid and
press together immediately. This cement will harden in 5 days.
III.—Graphite 50 pounds
Whiting 15 pounds
Litharge 15 pounds
Make to a paste with a boiled oil.
IV.—Make a paste of white lead and asbestos.
V.—Make a paste of litharge and glycerine. Red lead may be added. This
also does for stone.
VI.—Make a paste of boiled oil of equal parts of white lead, pipe clay,
and black oxide of manganese.
VII.—Make iron filings to a paste with water glass.
VIII.—Sal ammoniac 4 ounces
Sulphur 2 ounces
Iron filings 32 ounces
Make as much as is to be used at once to a paste with a little water.
This remark applies to both the following dry recipes:
IX.—Iron filings 160 ounces
Lime 80 ounces
Red lead 16 ounces
Alum 8 ounces
Sal ammoniac 2 ounces
X.—Clay 10 ounces
Iron filings 4 ounces
Salt 1 ounce
Borax 1 ounce
Black oxide of manganese 2 ounces
XI.—Mix:
Iron filings 180 ounces
Lime 45 ounces
Salt 8 ounces
XII.—Mix:
Iron filings 140 ounces
Hydraulic lime 20 ounces
Sand 25 ounces
Sal ammoniac 3 ounces
Either of these last two mixtures is made into a paste with strong
vinegar just before use.
XIII.—Mix equal weights of zinc oxide and black oxide of manganese into
a paste with water glass.
XIV.—Copal varnish, 15 parts; hydrated lime, 10 parts; glue _de
nerfs_ (of sinews), 5 parts; fat drying oil, 5 parts; {25} powdered
turpentine, 3 parts; essence of turpentine, 2 parts. Dissolve the
glue _de nerfs_ on the water bath, add all the other substances, and
triturate intimately.
XV.—Copal varnish, 15 parts; powdered turpentine, 3 parts; essence
of turpentine, 2 parts; powdered fish glue, 3 parts; iron filings, 3
parts; ocher, 10 parts.
XVI.—To make a cement for cast iron, take 16 ounces cast-iron borings;
2 ounces sal ammoniac, and 1 ounce sulphur. Mix well and keep dry.
When ready to use take 1 part of this powder to 20 parts of cast-iron
borings and mix thoroughly into a stiff paste, adding a little water.
XVII.—Litharge 2 parts
Boiled linseed oil 2 parts
White lead 1 part
Copal 1 part
Heat together until of a uniform consistence and apply warm.
XVIII.—A cement for iron which is said to be perfectly waterproof and
fireproof is made by working up a mixture of equal weights of red lead
and litharge with glycerine till the mass is perfectly homogeneous and
has the consistency of a glazier’s putty. This cement is said to answer
well, even for very large iron vessels, and to be unsurpassable for
stopping up cracks in large iron pans of steam pipes.
«Cement for Metal, Glass, and Porcelain.»—A soft alloy is prepared by
mixing from 30 to 36 parts of copper precipitated in the form of a
fine brown powder, with sulphuric acid of a specific gravity of 1.85
in a cast-iron or porcelain mortar and incorporating by stirring with
75 parts of mercury, the acid being afterwards removed by washing with
water. In from 10 to 14 hours the amalgam becomes harder than tin, but
when heated to 692° F., it can be kneaded like wax. In this condition
it is applied to the surface to be cemented, and will fix them firmly
together on cooling.
Dissolve 1 drachm of gum mastic in 3 drachms of spirits of wine. In
a separate vessel containing water soak 3 drachms of isinglass. When
thoroughly soaked take it out of the water and put it into 5 drachms
of spirits of wine. Take a piece of gum ammoniacum the size of a large
pea and grind it up finely with a little spirits of wine and isinglass
until it has dissolved. Then mix the whole together with sufficient
heat. It will be found most convenient to place the vessel on a
hot-water bath. Keep this cement in a bottle closely stoppered, and
when it is to be used, place it in hot water until dissolved.
«Cements for Fastening Porcelain to Metal.»—I.—Mix equal parts of
alcohol (95 per cent) and water, and make a paste by incorporating
the liquid with 300 parts of finely pulverized chalk and 250 parts of
starch.
II.—Mix finely powdered burned lime, 300 parts, with powdered starch,
250 parts, and moisten the mixture with a compound of equal parts of
water and alcohol of 95 per cent until a paste results.
III.—Cement or plaster can be used if the surfaces are sufficiently
large; cement is the better article when the object may be exposed
to moisture or subjected to much pressure. A process which can be
recommended consists in mingling equal weights of chalk, brickdust,
clay, and Romain cement. These materials, pulverized and sifted are
incorporated with linseed oil in the proportion of half a kilo of oil
to 3 kilos of the mingled powder. The Romain or Romanic cement is so
designated from the district in France where the calcareous stone from
which it is prepared is found in considerable quantity. Although its
adhesive qualities are unquestioned, there are undoubtedly American
cements equally as good.
IV.—Acetate of lead, 46 1/2 parts by weight; alum, 46 1/2 parts by
weight; gum arabic, 76 parts by weight; flour, 500 parts by weight;
water, 2,000 parts by weight. Dissolve the acetate of lead and the alum
in a little water; on the other hand dissolve the gum arabic in water
by pouring, for instance, the 2 liters of boiling water on the gum
arabic reduced to powder. When the gum has dissolved, add the flour,
put all on the fire, and stir well with a piece of wood; then add the
solution of acetate of lead and the alum; agitate well so as to prevent
any lumps from forming; retire from the fire before allowing to boil.
This glue is used cold, does not peel off, and is excellent to make
wood, glass, cardboard, etc. adhere to metals.
«Cement for Leather and Iron.»—To face a cast-iron pulley with leather
apply acetic acid to the face of the pulley with a brush, which will
roughen it by rusting, and then when dry apply a cement made of 1 pound
of fish glue and 1/2 pound of common glue, melted in a mixture of
alcohol and water. The leather should then be placed on the pulley and
dried under pressure. {26}
«Amber Cements.»—I.—To solder together two pieces of yellow amber,
slightly heat the parts to be united and moisten them with a solution
of caustic soda; then bring the two pieces together quickly.
II.—Dissolve in a closed bottle 75 parts of cut-up caoutchouc in 60
parts of chloroform. Add 15 parts of mastic and let the mixture stand
in the cold until all has dissolved.
III.—Moisten the pieces to be joined with caustic potash and press
them together when warm. The union is so perfect that no trace of the
juncture is visible. A concentrated alcoholic solution of the rosin
over the amber, soluble in alcohol, is also employed for this purpose.
Another medium is a solution of hard and very finely powdered copal in
pure sulphuric ether. Coat both fractures, previously well cleaned,
with this solution and endeavor to combine them intimately by tying or
pressing.
IV.—In 30 parts by weight of copal dissolve 30 parts by weight of
alumina by means of a water bath. Bathe the surface to be cemented with
this gelatinous liquid, but very slightly. Unite the fractures and
press them together firmly until the mixture is dry.
«Acid-Proof Cements for Stoneware and Glass.»—I.—Mix with the aid of
heat equal weights of pitch, rosin, and plaster of Paris.
II.—Mix silicate of soda to a paste with ground glass.
III.—Mix boiled oil to a paste with china clay.
IV.—Mix coal tar to a paste with pipe clay.
V.—Mix boiled oil to a paste with quicklime.
VI.—Mix with the aid of heat: Sulphur, 100 pounds; tallow, 2 pounds;
rosin, 2 pounds. Thicken with ground glass.
VII.—Mix with the aid of heat: Rosin, 2 pounds; sulphur, 2 pounds;
brickdust, 4 pounds.
VIII.—Mix with the aid of heat 2 pounds of india rubber and 4 pounds of
oiled oil. Thicken with 12 pounds of pipe clay.
IX.—Fuse 100 pounds of india rubber with 7 pounds of tallow. Then make
to a paste with dry slaked lime and finally add 20 pounds of red lead.
X.—Mix with the aid of heat: Rosin, 24 pounds; red ocher, 8 pounds;
boiled oil, 2 pounds; plaster of Paris, 4 pounds.
«Acid-Proof Cement for Wood, Metals, etc.»—
I.—Powdered asbestos 2 parts
Ground baryta 1 part
Sodium water-glass solution 2 parts
Mix.
II.—To withstand hot nitric acid the following is used:
Sodium water-glass solution 2 parts
Sand 1 part
Asbestos 1 part
Mix.
III.—Asbestos 2 parts
Sulphate of barium 3 parts
Silicate of sodium 2 parts
By mixing these ingredients a cement strong enough to resist the
strongest nitric acid will be obtained.
IV.—If hot acids are dealt with, the following mixture will be found to
possess still more resistant powers:
Silicate of sodium (50° Baumé) 2 parts
Fine sand 1 part
Asbestos 1 part
Both these cements take a few hours to set. If the cement is wanted to
set at once, use silicate of potassium, instead of silicate of sodium.
This mixture will be instantly effective and possesses the same power
of resistance as the other.
«Directions for Repairing Broken Glass, Porcelain, Bric-à-Brac.»—Broken
glass, china, bric-à-brac, and picture frames, not to name casts,
require each a different cement—in fact, several different cements.
Glass may be beautifully mended to look at, but seldom so as to be
safely used. For clear glass the best cement is isinglass dissolved in
gin. Put 2 ounces of isinglass in a clean, wide-mouthed bottle, add
half a pint of gin, and set in the sun until dissolved. Shake well
every day, and before using strain through double lawn, squeezing very
gently.
Spread a white cloth over the mending table and supply it with plenty
of clean linen rags, strong rubber bands, and narrow white tape,
also a basin of tepid water and a clean soft towel. Wash the broken
glass very clean, especially along the break, but take care not to
chip it further. Wet both broken edges well with the glue, using a
camel’s-hair pencil. Fit the break to a nicety, then slip on rubber
bands length- and cross-wise, every way they will hold. If they will
not hold true as upon a stemmed {27} thing, a vase or jug or scent
bottle, string half a dozen bands of the same size and strength upon a
bit of tape, and tie the tape about neck or base before beginning the
gluing. After the parts are joined slip another tape through the same
bands and tie it above the fracture; thus with all their strength the
bands pull the break together. The bands can be used thus on casts of
china—in fact, to hold anything mendable. In glass mending the greater
the pressure the better—if only it stops short of the breaking point.
Properly made the isinglass cement is as clear as water. When the
pieces fit true one on the other the break should be hardly visible, if
the pressure has been great enough to force out the tiny bubbles, which
otherwise refract the light and make the line of cleavage distressingly
apparent. Mended glass may be used to hold dry things—as rose leaves,
sachets, violet powder, even candies and fruits. But it will not bear
to have any sort of liquid left standing in it, nor to be washed beyond
a quick rinsing in tepid water. In wiping always use a very soft towel,
and pat the vessel dry with due regard to its infirmities.
Mend a lamp loose in the collar with sifted plaster of Paris mixed to a
very soft paste with beaten white of egg. Have everything ready before
wetting up the plaster, and work quickly so it may set in place. With
several lamps to mend wet enough plaster for one at a time. It takes
less than 5 minutes to set, and is utterly worthless if one tries
working it over. Metal work apart from the glass needs the soldering
iron. Dust the break well with powdered rosin, tie the parts firmly
together, lay the stick of solder above the break, and fetch the iron
down on it lightly but firmly. When the solder cools, remove the melted
rosin with a cloth dipped in alcohol.
Since breakables have so unhappy a knack of fracturing themselves in
such fashion they cannot possibly stand upright, one needs a sand box.
It is only a box of handy size with 8 inches of clean, coarse sand in
the bottom. Along with it there should be some small leaden weights,
with rings cast in them, running from an ounce to a quarter pound. Two
of each weight are needed. In use, tapes are tied to the rings, and
the pair of weights swung outside the edges of the box, so as to press
in place the upper part of a broken thing to which the tapes have been
fastened.
Set broken platters on edge in the sand box with the break up. The
sand will hold them firm, and the broken bit can be slapped on. It
is the same with plates and saucers. None of these commonly requires
weighting. But very fine pieces where an invisible seam is wanted
should be held firm until partly set, then have the pair of heaviest
weights accurately balanced across the broken piece. The weights are
also very useful to prop and stay topheavy articles and balance them so
they shall not get out of kilter. A cup broken, as is so common with
cups, can have the tape passed around it, crossing inside the handle,
then be set firmly in the sand, face down, and be held by the hanging
weights pulling one against the other.
The most dependable cement for china is pure white lead, ground
in linseed oil, so thick it will barely spread smoothly with a
knife. Given time enough to harden (some 3 months), it makes a seam
practically indestructible. The objection to it is that it always shows
in a staring white line. A better cement for fine china is white of egg
and plaster. Sift the plaster three times and tie a generous pinch of
it loosely in mosquito netting. Then beat the egg until it will stick
to the plaster. Have the broken edge very clean, cover both with the
beaten egg, dust well with the plaster, fit together at once, tie,
using rubber bands if possible, wrap loosely in very soft tissue paper,
and bury head and ears in the sand box, taking care that the break lies
so that the sand will hold it together. Leave in the box 24 hours.
After a week the superfluous plaster may be gently scraped away.
«General Formulas for Cements for Repairing Porcelain, Glassware,
Crockery, Plaster, and Meerschaum.»—I.—An excellent cement for joining
broken crockery and similar small articles can be made by melting 4 or
5 parts of rosin (or, better still, gum mastic) with 1 part of beeswax
in an iron spoon or similar vessel. Apply while hot. It will not stand
great heat.
II.—An excellent cement for porcelain and stoneware is obtained by
mixing 20 parts of fish glue with an equal weight of crystallizable
acetic acid and evaporate the mixture carefully to a syrupy consistency
so that it forms a gelatinous mass on cooling. For use the cement thus
obtained is made liquid again by heating and applied to the fracture
with a brush. The pieces should now be pressed firmly together, by
winding a twine tightly around them, until the cement has hardened.
III.—For luting vessels made of glass, {28} porcelain, etc., which
are to be used to hold strong acids, a mixture of asbestos powder,
water glass, and an indifferent powder (permanent white, sand, etc.)
is recommended. To begin with, asbestos powder is made into a pulp
with three or four times the quantity (weight) of a solution of soda
water glass (of 30° B.). The same is exceedingly fat and plastic, but
is not very well suited for working, as it shrinks too much and cracks
when drying. By an addition of fine writing sand of the same weight
as the asbestos used, the mass can be made less fat, so as to obviate
shrinking, without detracting from the plasticity. Small vessels were
molded from it and dried in the air, to be tested afterwards. Put in
water, the hardened mass becomes soft again and falls apart. Brought
into contact, however, with very strong mineral acids, it becomes even
firmer and withstands the liquid perfectly. Concentrated nitric acid
was kept in such small vessels without the mass being visibly attacked
or anything penetrating it. The action of the acid manifestly has the
effect that silicic acid is set free from the water glass in excess,
which clogs up the pores entirely and contributes to the lutation.
Later on, the mass cannot be dissolved by pure water any more. The mass
is also highly fireproof. One of the molded bodies can be kept glowing
in a Bunsen gas flame for about half a day after treatment with acid,
without slagging in the least. For many purposes it ought to be welcome
to have such a mass at hand. It cannot be kept ready for use, however,
as it hardens a few hours after being prepared; if potash water glass
is used, instead of the soda composition, this induration takes place
still more quickly.
IV.—Cement for Glass, Porcelain, etc.—
Isinglass (fish glue) 50 parts
Gum ammoniac 4 parts
Gum mastic 2 parts
Alcohol, 95 per cent 10 parts
Water, q. s.
Soak the isinglass in cold water over night, or until it has become
swollen and soft throughout. In the morning throw off any superfluous
fluid and throw the isinglass on a clean towel or other coarse cloth,
and hang it up in such a way that any free residual water will drain
away. Upon doing this thoroughly depends, in a great measure, the
strength of the cement. When the gelatin has become thoroughly drained
put it into a flask or other container, place it in the water bath and
heat carefully until it becomes fluid, being careful not to let it come
to a boil, as this injures its adhesive properties (the same may be
said in regard to glues and gelatins of all kinds). Dissolve the gums
in the alcohol and add the solution to the gelatin after removing the
same from the water bath, and letting it cool down to about 160° F.
Stir well together or mix by agitation.
The following precautions must be observed: 1. Both surfaces to be
joined must be absolutely clean, free from dust, dirt, grease, etc.
2. Where the cement is one that requires the application of heat
before use, the objects to be united should also _be heated to a point
at least as high as the melting point of the cement_. Otherwise, the
cement on application is chilled and consequently fails to make a
lasting joint. 3. The thinner the layer of cement the stronger the
joint; avoid, therefore, using too much of the binding material. Cover
both surfaces to be united, coapt them exactly, and press together as
closely as possible. In this manner the thinnest possible layer is
secured. 4. Bind the parts securely together, and let remain without
loosening or attempting to use the article for 2 or 3 days or longer. A
liquid cement acquires its full strength only after evaporation of the
fluids used as solvents, and this can occur only from the infinitesimal
line of exposed surface.
V.—Liquid Porcelain Cement.—Fish glue, 20 parts; glass acetic acid, 20
parts; heat together until the mass gelatinizes on cooling.
VI.—Take 1 ounce of Russian isinglass, cut in small pieces, and bruise
well; then add 6 ounces of warm water, and leave it in a warm place
for from 24 to 48 hours. Evaporate the resulting solution to about 3
ounces. Next dissolve 1/2 ounce of mastic in 4 ounces of alcohol,
and add the mastic solution to the isinglass in small quantities at a
time, continuing the heat and stirring well. While still hot strain the
liquid through muslin.
VII.—For optical glasses, Canada balsam is employed, the two pieces
being firmly pressed together. After a while, especially by humidity,
punctures will form, and the glass is separated by a mist of varying
reflexes, while in certain climates the heat will melt the balsam. For
all other glass articles which require only simple treatment, such as
knobs of covers, plates, etc., silicate of potash is excellent.
VIII.—Glass Cement.—Dissolve in 150 parts of acetic acid of 96 per
cent, 100 {29} parts of gelatin by the use of heat, and add ammonium
bichromate, 5 parts. This glue must be kept away from the light.
IX.—White glue 10 parts
Potassium bichromate 2 parts
Water 100 parts
The glue is dissolved in a portion of the water by the aid of heat,
the bichromate in the remainder, and the liquids mixed, the mixing
being done in a feebly lighted place, and the mixture is then kept
in the dark. It is applied in feeble light, being reliquefied by
gentle heat, and the glass, the fractured pieces being tightly clamped
together, is then exposed to a strong light for some time. By this
exposure the cement becomes insoluble. This is waterproof cement for
glass.
X.—Diamond Glass Cement.—Dissolve 100 parts of fish glue in 150 parts
of 90 per cent alcohol and add, with constant stirring, 200 parts of
powdered rosin. This cement must be preserved in absolutely tight
bottles, as it solidifies very quickly.
XI.—To unite objects of crystal dissolve 8 parts of caoutchouc and 100
parts of gum mastic in 600 parts of chloroform. Set aside, hermetically
closed, for 8 days; then apply with a brush, cold.
XII.—To make a transparent cement for glass, digest together for a week
in the cold 1 ounce of india rubber, 67 ounces of chloroform, and 40
ounces of mastic.
XIII.—A mixture of traumaticin, a solution of caoutchouc in chloroform,
and a concentrated solution of water glass make a capital cement for
uniting articles of glass. Not only is the joint very strong, but it
is transparent. Neither changes of temperature nor moisture affect the
cement.
XIV.—A transparent cement for porcelain is prepared by dissolving 75
parts of india rubber, cut into small pieces, in a bottle containing
60 parts chloroform; to this add 15 parts green mastic. Let the
bottle stand in the cold until the ingredients have become thoroughly
dissolved.
XV.—Some preparations resist the action of heat and moisture a short
time, but generally yield very quickly. The following cement for glass
has proven most resistant to liquids and heat:
Silver litharge 1,000 parts
White lead 50 parts
Boiled linseed oil 3 parts
Copal varnish 1 part
Mix the lead and litharge thoroughly, and the oil and copal in the
same manner, and preserve separately. When needed for use, mix in
the proportions indicated (150 parts of the powder to 4 parts of the
liquid) and knead well together. Apply to the edges of the glass, bind
the broken parts together, and let stand for from 24 to 48 hours.
XVI.—To reunite plaster articles dissolve small pieces of celluloid in
ether; in a quarter of an hour decant, and use the pasty deposit which
remains for smearing the edges of the articles. It dries rapidly and is
insoluble in water.
XVII.—To Mend Wedgwood Mortars.—It is easy enough to mend mortars so
that they may be used for making emulsions and other light work which
does not tax their strength too much. But a mended mortar will hardly
be able to stand the force required for powdering hard substances. A
good cement for mending mortars is the following:
_a._—Glass flour elutriated 10 parts
Fluorspar, powdered and elutriated 20 parts
Silicate of soda 60 parts
Both glass and fluorspar must be in the finest possible condition,
which is best done by shaking each in fine powder, with water allowing
the coarser particles to deposit, and then to pour off the remainder,
which holds the finest particles in suspension. The mixture must be
made very rapidly by quick stirring, and when thoroughly mixed must be
at once applied. This is said to yield an excellent cement.
_b._—Freshly burnt plaster of Paris 5 parts
Freshly burnt lime 1 part
White of egg, sufficient.
Reduce the first two ingredients to a very fine powder and mix them
well; moisten the two surfaces to be united with a small quantity of
white of egg to make them adhesive; then mix the powder very rapidly
with the white of egg and apply the mixture to the broken surfaces. If
they are large, two persons should do this, each applying the cement
to one portion. The pieces are then firmly pressed together and left
undisturbed for several days. The less cement is used the better will
the articles hold together.
_c._—If there is no objection to dark-colored cement, the very best
that can be used is probably marine glue. This is made thus: Ten parts
of caoutchouc or india rubber are dissolved in 120 parts of benzine
or petroleum naphtha, with {30} the aid of a gentle heat. When the
solution is complete, which sometimes requires from 10 to 14 days,
20 parts of asphalt are melted in an iron vessel and the caoutchouc
solution is poured in very slowly in a fine stream and under continued
heating, until the mass has become homogeneous and nearly all the
solvent has been driven off. It is then poured out and cast into
greased tin molds. It forms dark brown or black cakes, which are very
hard to break. This cement requires considerable heat to melt it; and
to prevent it from being burnt it is best to heat a capsule containing
a piece of it first on a water bath until the cake softens and begins
to be liquid. It is then carefully wiped dry and heated over a naked
flame, under constant stirring, up to about 300° F. The edges of the
article to be mended should, if possible, also be heated to at least
212° F., so as to permit the cement to be applied at leisure and with
care. The thinner the cement is applied the better it binds.
«Meerschaum Cements.»—I.—If the material is genuine (natural)
meerschaum a lasting joint can be made between the parts by proceeding
as follows: Clean a clove or two of garlic (the fresher the better) by
removing all the outside hull of skin; throw into a little mortar and
mash to a paste. Rub this paste over each surface to be united and join
quickly. Bring the parts as closely together as possible and fasten in
this position. Have ready some boiling fresh milk; place the article in
it and continue the boiling for 30 minutes. Remove and let cool slowly.
If properly done, this makes a joint that will stand any ordinary
treatment, and is nearly invisible. For composition, use a cement made
of quicklime, rubbed to a thick cream with egg albumen.
II.—Mix very fine meerschaum shavings with albumen or dissolve casein
in water glass, stir finely powdered magnesia into the mass, and use
the cement at once. This hardens quickly.
«Asbestos Cement.»—Ground asbestos may be made into a cement which
will stand a high degree of heat by simply mixing it with a solution
of sodium silicate. By subsequent treatment with a solution of calcium
chloride the mass may be made insoluble, silicate of calcium being
formed.
A cement said to stand a high degree of heat and to be suitable for
cementing glass, porcelain, or other vessels intended to hold corrosive
acids, is this one:
I.—Asbestos 2 parts
Barium sulphate 3 parts
Sodium silicate 2 parts
By mixing these ingredients a cement strong enough to resist the
strongest nitric acid will be obtained. If hot acids are dealt with,
the following mixture will be found to possess still more resistant
powers:
II.—Sodium silicate 2 parts
Fine sand 1 part
Asbestos powder 1 part
Both these cements take a few hours to set. If the cement is wanted to
set at once, use potassium silicate instead of sodium silicate. This
mixture will be instantly effective, and possesses the same power of
resistance as the other.
«Parisian Cement.»—Mix 1 part of finely ground glass powder, obtained
by levigation, with 3 parts of finely powdered zinc oxide rendered
perfectly free from carbonic acid by calcination. Besides prepare a
solution of 1 part, by weight, of borax in a very small quantity of
hot water and mix this with 50 parts of a highly concentrated zinc
chloride solution of 1.5 to 1.6 specific gravity. As is well known the
mixture of this powder with the liquid into a soft uniform paste is
accomplished only immediately before use. The induration to a stonelike
mass takes place within a few minutes, the admixture of borax retarding
the solidification somewhat. The pure white color of the powder may be
tinted with ocher, manganese, etc., according to the shade desired.
«Strong Cement.»—Pour over well-washed and cleaned casein 12 1/2
parts of boiled linseed oil and the same amount of castor oil. Boil.
Stir actively and add a small amount of a saturated aqueous solution of
alum; remove from the fire and set aside. After a while a milky looking
fluid will separate and rise. This should be poured off. To the residue
add 120 parts of rock candy syrup and 6 parts of dextrin.
«A Cheap and Excellent Cement.»—A cheap and excellent cement, insoluble
after drying in water, petroleum, oils, carbon disulphide, etc., very
hard when dry and of very considerable tensile strength, is composed
of casein and some tannic-acid compound, as, for instance, calcium
tannate, and is prepared as follows:
First, a tannin solution is prepared either by dissolving a tannin
salt, or by extraction from vegetable sources (as barks from certain
trees, etc.), to which {31} is added clear lime water (obtained by
filtering milk of lime, or by letting the milk stand until the lime
subsides) until no further precipitation occurs, and red litmus paper
plunged in the fluid is turned blue. The liquid is now separated
from its precipitate, either by decantation or otherwise, and the
precipitate is dried. In operating with large quantities of the
substance, this is done by passing a stream of atmospheric air through
the same. The lime tannate obtained thus is then mixed with casein in
proportions running from 1:1 up to 1:10, and the mixture, thoroughly
dried, is milled into the consistency of the finest powder. This
powder has now only to be mixed with water to be ready for use, the
consistency of the preparation depending upon the use to which it is to
be put.
«Universal Cement.»—Take gum arabic, 100 parts, by weight; starch, 75
parts, by weight; white sugar, 21 parts, by weight; camphor, 4 parts,
by weight. Dissolve the gum arabic in a little water; also dissolve the
starch in a little water. Mix and add the sugar and camphor. Boil on
the water bath until a paste is formed which, on coating, will thicken.
«Cement for Ivory.»—Melt together equal parts of gutta percha and
ordinary pitch. The pieces to be united have to be warmed.
«Cement for Belts.»—Mix 50 parts, by weight, of fish glue with equal
parts of whey and acetic acid. Then add 50 parts, by weight, of garlic
in paste form and boil the whole on the water bath. At the same time
make a solution of 100 parts, by weight, of gelatin in the same
quantity of whey, and mix both liquids. To the whole add, finally,
50 parts, by weight, of 90-per-cent alcohol and, after filtration,
a cement is obtained which can be readily applied with a brush and
possesses extraordinary binding qualities.
«Cement for Chemical Apparatus.»—Melt together 20 parts of gutta
percha, 10 parts of yellow wax, and 30 parts of shellac.
«Size Over Portland Cement.»—The best size to use on Portland cement
molding for wall paper would ordinarily be glue and alum size put on
thin and warm, made in proportion of 1/2 pound of glue and same
weight of alum dissolved in separate pails, then poured together.
«Aquarium Cements.»—
I.—Litharge 3 ounces
Fine white sand 3 ounces
Plaster of Paris 3 ounces
Rosin, in fine powder 1 ounce
Linseed oil, enough.
Drier, enough.
Mix the first three ingredients, add sufficient linseed oil to make a
homogeneous paste, and then add a small quantity of drier. This should
stand a few hours before it is used. It is said that glass joined to
iron with this cement will break before it will come loose.
II.—Litharge 1 ounce
Fine white sand 1 ounce
Plaster of Paris 1 ounce
Manganese borate 20 grains
Rosin, in fine powder 3 1/2 pounds
Linseed varnish oil, enough.
III.—Take equal parts of flowers of sulphur, ammonium chloride, and
iron filings, and mix thoroughly with boiled linseed oil. Finally, add
enough white lead to form a thin paste.
IV.—Powdered graphite 6 parts
Slaked lime 3 parts
Barium sulphate 8 parts
Linseed varnish oil 7 parts
V.—Simply mix equal parts of white and red lead with a little
kettle-boiled linseed oil.
«Substitute for Cement on Grinder Disks.»—A good substitute in place of
glue or various kinds of cement for fastening emery cloth to the disks
of grinders of the Gardner type is to heat or warm the disk and apply a
thin coating of beeswax; then put the emery cloth in place and allow to
set and cool under pressure.
«Knockenplombe.»—If 1 part of thymol be mixed with 2 parts of iodoform
we obtain a substance that retains its fluidity down to 72° C.
(161.6° F.). If the temperature be carried down to 60° C. (140° F.)
it suddenly becomes solid and hard. If, in its liquid condition, this
substance be mixed intimately with an equal quantity of calcined bone,
it forms a cement that can be molded or kneaded into any shape, that,
at the temperature of the body (98° F.), becomes as hard as stone, a
fact that suggests many useful purposes to which the mixture may be put.
«Cement for General Use.»—Take gum arabic, 100 parts, by weight;
starch, 75 {32} parts by weight; white sugar, 21 parts, by weight;
camphor, 4 parts, by weight. Dissolve the gum arabic in a little water.
On the other hand, dissolve the starch also in some water. When this is
done add the sugar and the camphor and put in a water bath. Boil until
a paste is formed, which must be rather thin, because it will thicken
on cooling.
«Strong Cement.»—Pour over well-washed and cleaned casein 12 1/2
parts of boiled linseed oil and the same amount of castor oil, put on
the fire and bring to a boil; stir actively and add a small amount of
a saturated aqueous solution of alum; remove from the fire and set
aside. After standing a while a milky-looking fluid will separate at
the bottom and rise to the top. This should be poured off and to the
residue add 120 parts of rock-candy syrup and 6 parts of dextrine.
«Syndeticon.»—I.—Slake 100 parts of burnt lime with 50 parts of water,
pour off the supernatant water; next, dissolve 60 parts of lump sugar
in 160 parts of water, add to the solution 15 parts of the slaked
lime, heat to 70° or 80° C. (158° to 176° F.), and set aside, shaking
frequently. Finally dissolve 50 to 60 parts of genuine Cologne glue in
250 parts of the clear solution.
II.—A solution of 10 parts gum arabic and 30 parts of sugar in 100
parts of soda water glass.
III.—A hot solution of 50 parts of Cologne glue in 60 parts of a
20-per-cent aqueous calcium-chloride solution.
IV.—A solution of 50 parts of Cologne glue in 60 parts of acetic acid.
V.—Soak isinglass (fish bladder) in acetic acid of 70 per cent until it
swells up, then rub it up, adding a little water during the process.
«“Shio Liao.”»—Under this name the Chinese manufacture an excellent
cement which takes the place of glue, and with which gypsum, marble,
porcelain, stone, and stoneware can be cemented. It consists of the
following parts (by weight): Slaked powdered lime, 54 parts; powdered
alum, 6 parts; and fresh, well-strained blood, 40 parts. These
materials are stirred thoroughly until an intimately bound mass of
the consistency of a more or less stiff salve is obtained. In paste
form this mass is used as cement; in a liquid state it is employed for
painting all sorts of articles which are to be rendered waterproof and
durable. Cardboard covers, which are coated with it two or three times,
become as hard as wood. The Chinese paint their houses with “shio liao”
and glaze their barrels with it, in which they transport oil and other
greasy substances.
«LUTES.»
Lutes always consist of a menstruum and dissolved or suspended solids,
and they must not be attacked by the gases and liquids coming in
contact with them. In some cases the constituents of the lute react to
form a more strongly adhering mass.
The conditions of application are, in brief:
(_a_) Heating the composition to make it plastic until firmly fixed in
place.
(_b_) Heating the surfaces.
(_c_) Applying the lute with water or a volatile solvent, which is
allowed to volatilize.
(_d_) Moistening the surfaces with water, oil, etc. (the menstruum of
the lute itself).
(_e_) Applying the lute in workable condition and the setting taking
place by chemical reactions.
(_f_) Setting by hydration.
(_g_) Setting by oxidation.
These principles will be found to cover nearly all cases.
Joints should not be ill-fitting, depending upon the lute to do what
the pipes or other parts of the apparatus should do. In most cases one
part of the fitting should overlap the other, so as to make a small
amount of the lute effective and to keep the parts of the apparatus
rigid, as a luted joint is not supposed to be a particularly strong
one, but rather one quickly applied, effective while in place and
easily removed.
Very moderate amounts of the lute should be used, as large amounts are
likely to develop cracks, be rubbed off, etc.
A classification may be given as follows:
(1) Plaster of Paris.
(2) Hydraulic cement.
(3) Clay.
(4) Lime.
(5) Asphalt and pitch.
(6) Rosin.
(7) Rubber.
(8) Linseed oil.
(9) Casein and albumen.
(10) Silicates of soda and oxychloride cements.
(11) Flour and starch.
(12) Miscellaneous, including core compounds.
I. Plaster of Paris is, of course, often used alone as a paste; which
quickly {33} solidifies, for gas and wood distillation retorts, etc.,
and similar places where quickness of setting is requisite. It is more
often, however, used with some fibrous material to give it greater
strength. Asbestos is the most commonly used material of these, as it
will stand a high temperature. When that is not so important, straw,
plush trimmings, hair, etc., are used as binders, while broken stone,
glass, and various mineral substances are used as fillers, but they do
not add anything to the strength. These lutes seem to be particularly
suitable for oil vapors and hydrocarbon gases.
Formulas:
(1) Plaster and water.
(2) Plaster (wet) and asbestos.
(3) Plaster (wet) and straw.
(4) Plaster (wet) and plush trimmings.
(5) Plaster (wet) and hair.
(6) Plaster (wet) and broken stone, etc.
II. Hydraulic Cement.—Cement is used either alone or with sand,
asbestos, etc. These lutes are suitable for nitric acid. When used
with substances such as rosin or sulphur, cement is probably employed
because it is in such a fine state of division and used as a filler and
not because of any powers of setting by hydration.
Formulas:
(1) Cement—neat.
(2) Cement and asbestos.
(3) Cement and sand.
III. Clay.—This most frequently enters into the composition of lutes as
a filler, but even then the very finely divided condition of certain
grades renders it valuable, as it gives body to a liquid, such as
linseed oil, which, unless stiffened, would be pervious to a gas,
the clay in all cases being neutral. Thus, for luting pipes carrying
chlorine, a stiff paste of clay and molasses has been suggested by
Theo. Köller in _Die Surrogate_, but it soon gives way.
Formulas:
(1) Clay and linseed oil.
(2) Same, using fire clay.
(3) Clay and molasses.
(1) Is suitable for steam, etc.; (2) for chlorine, and (3) for oil
vapors.
IV. Lime is used in the old lute known as putty, which consists of
caustic lime and linseed oil. Frequently the lime is replaced by chalk
and china clay, but the lime should be, in part at least, caustic, so
as to form a certain amount of lime soap. Lime is also used in silicate
and casein compositions, which are very strong and useful, but will be
described elsewhere.
Formulas:
(1) Lime and boiled oil to stiff mass.
(2) Clay, etc., boiled oil to stiff mass.
V. Asphalt and Pitch.—These substances are used in lutes somewhat
interchangeably. As a rule, pitch makes the stronger lutes. Tar is
sometimes used, but, because of the light oils and, frequently, water
contained, it is not so good as either of the others.
Asphalt dissolved in benzol is very useful for uniting glass for
photographic, microscopical, and other uses. Also for coating wood,
concrete, etc., where the melted asphalt would be too thick to cover
well. Benzol is the cheapest solvent that is satisfactory for this
purpose, as the only one that is cheaper would be a petroleum naphtha,
which does not dissolve all the constituents of the asphalt. For
waterproofing wood, brick, concrete, etc., melted asphalt alone is
much used, but when a little paraffine is added, it improves its
waterproofing qualities, and in particular cases boiled oil is also
added to advantage.
Formulas:
1. Refined lake asphalt.
2. Asphalt 4 parts
Paraffine 1 part
3. Asphalt 10 parts
Paraffine 2 parts
Boiled oil 1 part
Any of these may be thinned with hot benzol or toluol. Toluol is
less volatile than benzol and about as cheap, if not cheaper, the
straw-colored grades being about 24 cents per gallon.
Examples of so-called “stone cement” are:
4. Pitch 8 parts
Rosin 6 parts
Wax 1 part
Plaster 1/4 to 1/2 part
5. Pitch 8 parts
Rosin 7 parts
Sulphur 2 parts
Stone powder 1 part
These compositions are used to unite slate slabs and stoneware for
domestic, engineering, and chemical purposes. Various rosin and pitch
mixtures are used for these purposes, and the proportions of these two
ingredients are determined by the consistency desired. Sulphur and
stone powder are added to prevent the formation of cracks, sulphur
acting chemically and stone powder mechanically. {34} Where the lute
would come in contact with acid or vapors of the same, limestone should
not be the powder used, otherwise it is about the best. Wax is a useful
ingredient to keep the composition from getting brittle with age.
A class of lutes under this general grouping that are much used are
so-called “marine glues” (q. v.). They must be tough and elastic. When
used for calking on a vessel they must expand and contract with the
temperature and not crack or come loose.
Formulas:
6. Pitch 3 parts
Shellac 2 parts
Pure crude rubber 1 part
7. Pitch 1 part
Shellac 1 part
Rubber substitute 1 part
These are used by melting over a burner.
VI. Rosin, Shellac, and Wax.—A strong cement, used as a stone cement,
is:
1. Rosin 8 parts
Wax 1 part
Turpentine 1 part
It has little or no body, and is used in thin layers.
For nitric and hydro
Cite this
"Henley's Twentieth Century Formulas, Recipes and Processes". Project Gutenberg. Public domain in the USA. https://www.gutenberg.org/ebooks/53143